TECHNET Archives

April 2010

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, Ioan Tempea <[log in to unmask]>
Date:
Thu, 1 Apr 2010 16:51:00 -0500
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Content-Transfer-Encoding:
quoted-printable
Subject:
From:
"David D. Hillman" <[log in to unmask]>
X-cc:
In-Reply-To:
Content-Type:
text/plain; charset="ISO-8859-1"
MIME-Version:
1.0
Parts/Attachments:
text/plain (115 lines)
Hi Ioan - take a look at the email archive describe by Steve G. - if the 
surface finish is bright acid tin then you may have an excess codeposited 
plating condition as was described during the Technet conversation on Joe 
Kane's question.

Dave Hillman
Rockwell Collins
[log in to unmask]




Ioan Tempea <[log in to unmask]> 
Sent by: TechNet <[log in to unmask]>
04/01/2010 01:37 PM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
Ioan Tempea <[log in to unmask]>


To
[log in to unmask]
cc

Subject
[TN] Grainy after wave






Dear Technos,

 

Please see photo at http://ipc-technet.groupsite.com/gallery/12732

 

The component is a high current fuse holder, see the vertical mini 
-powerclaw, Sn over Ni finish 
http://www.andersonpower.com/products/pcb-powerclaw.html

 

We wave it with SN100C, 525F solder temperature, water soluble flux. As 
you notice, the finish on the left contact turns grainy, compared to the 
one next to it, that keeps the same look as before wave. The copper plane 
connections of the 2 contacts are different, hence a temperature 
differential between the 2.

 

My questions are:

How this happens? Sn starting reacting with the underlying Ni?

Should I worry about this? After all it is only a superficial issue. Can 
it alter the functionality of the contacts (they are supposed to see a lot 
of Amps)?

 

Thanks,

 

Ioan Tempea, ing.
Ingénieur Principal de Fabrication / Senior Manufacturing Engineer
T | 450.967.7100 ext.244
E | [log in to unmask] <mailto:[log in to unmask]> 
W | www.digico.cc <http://www.digico.cc/> 

 
 N'imprimer que si nécessaire - Print only if you must

 


______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to 
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 
for additional information, or contact Keach Sasamori at [log in to unmask] or 
847-615-7100 ext.2815
-----------------------------------------------------


______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2