I have had a very similar as Bev issue come up here, only in this case it has to do with the absence of a heel fillet on a completely plated part. My question is this: Does the lead forming angle play a role in whether or not a heel fillet forms when a part is soldered to the pad?
We have a fine pitch QFP device (19 mil pitch) that we are soldering at SMT. Our quality department is rejecting the boards because of a absence of a visible heel fillet per IPC 610D class 3. When I look at an unsoldered part under the scope, the angle between the foot and the leg is damn close to 90 degrees!
We are using a 5 mil thick stencil with 1 mil reduction on the width and 1:1 in the length, resulting in a 2-3 mil actual solder height (after the flux has blown off). Has anyone seen a scenario that prevents the solder from wicking up the foot to the leg forming a heel fillet because of the forming angle? I am also looking to see if a possible contamination issue on the part can result in this phenomenon.
Thanks,
Amol
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Bev Christian
Sent: Tuesday, March 30, 2010 9:24 PM
To: [log in to unmask]
Subject: Re: [TN] Need some opinions
Dave,
A distinction has to be made between failing the SMT process and failing the
product. Obviously the issue has little to do with screen printing,
placement or reflow - all other parts have the proper amount of solder
paste, are placed properly, have good looking joints and intermetallic of an
appropriate thickness is there, even on the leaded component in question
(where there is an actual joint!). So the process is in control.
With regards to the two other component types, I have some comments. SOIC
sheared toes have been a pain for quite some time. However, we already know
that toe fillets only provide 5% of joint strength at most and industry
available reliability data certainly shows that absence of toe fillets on
leaded components is not something to be overly concerned about. OK, let's
discuss LGAs and QFNs with sawn vertical surfaces.
1) The easiest way to avoid bulbous joints with these components is
tight control of pad size and the amount of solder paste deposited.
2) If negative wetting angles are produced, they are not pointed in
the direction where it can do the most damage. They point straight down
into the bulk of the solder. Negative wetting angles at the heel fillet of
a leaded device are pointing right down or close to the intermetallic
demarcation line.
3) We have never seen a bulbous joint of a LGA or QFN on a rigid board
cause a failure during thermal cycling, drop or tumble.
4) However, we do not allow bulbous joints on these devices on flex
circuits. I'll let everyone think about that one. Maybe we are over
cautious, but.
Bev
RIM
_____
From: [log in to unmask] [mailto:[log in to unmask]]
Sent: Tuesday, March 30, 2010 5:30 PM
To: TechNet E-Mail Forum; Bev Christian
Cc: [log in to unmask]
Subject: Re: [TN] Need some opinions
Hi Bev - I wouldn't "fail" the soldering process or the solder joint if I
can show the reason is the lack of plating "by design" as you described.
However, as other folks have pointed out, there are other functional issues
having a SMT component lead sufficiently plated which need to be considered.
The industry is already starting to ask the same questions in terms of have
sheared toes (SOIC type components) or sawed surfaces (QFN type components)
but those cases are not as severe as your case.
Dave Hillman
Rockwell Collins
[log in to unmask]
Bev Christian <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
03/25/2010 08:08 PM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
Bev Christian <[log in to unmask]>
To
[log in to unmask]
cc
Subject
[TN] Need some opinions
Technetters,
It seems that more and more component suppliers are not plating their leads
all the way up to the component body. In fact some are getting downright
skimpy and only plating to the bottom bend, never mind the upper one. If you
put down a lot of solder paste you end up with a bulbous joint, a negative
wetting angle and a stress concentration point. If you put down less paste
and have a co-planarity issue, then you have the potential for opens. The
other option of course is getting the supplier to plate higher up the leads.
Question: would you consider the condition of the formation of the negative
wetting angles a failure during process qualification?
Bev
RIM
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
WARNING: Export Control
This document may contain technical data within the definition of the
International Traffic in Arms Regulations (ITAR), and subject to the Export
Control Laws of the U.S. Government. Transfer of such data by any means to a
foreign person, whether in the United States or abroad, without proper export
authorization or other approval from the U.S. Department of State is
prohibited.
CONFIDENTIALITY NOTICE:
This e-mail, and any attachments, is for the sole use of the intended
recipient(s) and may contain information that is confidential and
protected from disclosure under the law. Any unauthorized review, use,
disclosure, or distribution is prohibited. If you are not the intended
recipient, please contact the sender by reply e-mail, and delete/destroy
all copies of the original message and attachments.
Thank you.
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|