TECHNET Archives

March 2010

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
Bev Christian <[log in to unmask]>, TechNet E-Mail Forum <[log in to unmask]>
Date:
Tue, 2 Mar 2010 12:03:41 -0500
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Chris Mahanna <[log in to unmask]>
Subject:
From:
Chris Mahanna <[log in to unmask]>
MIME-Version:
1.0
In-Reply-To:
Content-Transfer-Encoding:
quoted-printable
Content-Type:
text/plain; charset="us-ascii"
Parts/Attachments:
text/plain (255 lines)
Hi Bev,

We did a horizontal section from the component side.

At least for this one particular sample there is a correlation between the columnar (square) joints and relatively less paste.  Thanks for the clue.

Dave, the bulbous joints appear to have too much paste, but not so much to short.  The columnar joints appear to stretch or maybe even retain the shape of the stencil.  I'm sure that the small board side lands, soldermask and surface tension play a role.  Unfortunately I've got to move on to the next project--inspecting hundreds of dip-and-look.

Chris   

 
-----Original Message-----
From: Bev Christian [mailto:[log in to unmask]] 
Sent: Monday, March 01, 2010 1:17 PM
To: TechNet E-Mail Forum; Chris Mahanna
Subject: RE: [TN] BTC rework, Square SJs

Chris,
I think you will find that this happens when a particular joint does not
have enough solder paste printed with respect to the rest of the joints.
There is enough solder so there is not an open or a head on pillow
(HoP), but not enough to give what we normally expect (slightly
bulbous).  The joint gets "stretched" and you end up with more or less
straight sides.
Bev
RIM

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Chris Mahanna
Sent: Monday, March 01, 2010 1:08 PM
To: [log in to unmask]
Subject: Re: [TN] BTC rework, Square SJs

In cross section, the vertical sides of the joint are straight.  I
assume it has more/less retained the shape of the [trapezoidal?]
stencil.
Chris

From: Werner Engelmaier [mailto:[log in to unmask]]
Sent: Monday, March 01, 2010 12:52 PM
To: [log in to unmask]; Chris Mahanna
Subject: Re: [TN] BTC rework, Square SJs

Chris,
What do you mean by "square joints?"
Werner


-----Original Message-----
From: Chris Mahanna <[log in to unmask]>
To: [log in to unmask]
Sent: Mon, Mar 1, 2010 12:15 pm
Subject: [TN] BTC rework, Square SJs

Are square joints simply due to the small mass of the components, or is
it





possibly an indicator of insufficient heat?  We have no indication that
any of





the paste didn't flow.  Wetting looks good.  All evidence is from
microsection.










Thanks,





Chris










______________________________________________________________________





This email has been scanned by the MessageLabs Email Security System.





For more information please contact helpdesk at x2960 or
[log in to unmask]<mailto:[log in to unmask]>





______________________________________________________________________










---------------------------------------------------





Technet Mail List provided as a service by IPC using LISTSERV 15.0





To unsubscribe, send a message to
[log in to unmask]<mailto:[log in to unmask]> with following text in





the BODY (NOT the subject field): SIGNOFF Technet





To temporarily halt or (re-start) delivery of Technet send e-mail to





[log in to unmask]<mailto:[log in to unmask]>: SET Technet NOMAIL or (MAIL)





To receive ONE mailing per day of all the posts: send e-mail to





[log in to unmask]<mailto:[log in to unmask]>: SET Technet Digest





Search the archives of previous posts at:
http://listserv.ipc.org/archives





Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for





additional information, or contact Keach Sasamori at
[log in to unmask]<mailto:[log in to unmask]> or





847-615-7100 ext.2815





-----------------------------------------------------










______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or
[log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------

---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful.

______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2