Hi Werner,
I didn't know you wanted me to post the picture last night, so I got it up now. It's at:
http://stevezeva.homestead.com/files/Werner_Buckle.jpg
I'm working swing shift now...
Steve
-----Original Message-----
From: Leadfree [mailto:[log in to unmask]] On Behalf Of Werner Engelmaier
Sent: Wednesday, February 03, 2010 9:41 AM
To: [log in to unmask]
Subject: Re: [LF] [TN] track lifting
Hi Everybody,
I sent Steve another 'buckle-up' trace lifting picture to put on his site. So now, together with Brian's case we have 3 documented occurrences.
So, please, as I wrote to Brian:
I would appreciate pictures, possibly also to Steve, that I could use in my
reliability column—this is a failure mode fairly new and unknown to most
people.
If you could, I also would appreciate the base material, the peak reflow
temperature, the cooling rate after reflow, the Cu trace thickness and whether
it was covered with solder, and what solder. I now, its asking a lot, but only
with all the pertinent info can we make sense of this.
Werner
-----Original Message-----
From: Stadem, Richard D. <[log in to unmask]>
To: TechNet E-Mail Forum <[log in to unmask]>; Werner Engelmaier <[log in to unmask]>
Sent: Wed, Feb 3, 2010 9:33 am
Subject: RE: [TN] track lifting
Like Steve, my first thoughts were that the BGA in the picture was apparently
impacted, or somehow lifted and then put back down and reflowed.
However if that had happened, it could not have happened without many other
traces on each side of the lifted ones also being lifted and damaged, but they
are not.
Therefore I agree with Werner, that this is a case of damage due to severe CTE
mismatch. I have never seen this before.
Burke, I'll take you up on that bet. I doubt that there will be any delamination
issues. This appears to be a case where the PWB expanded and shrunk back in the
X and Y axis during reflow or temperature cycling, but I doubt that it saw any
significant Z-axis expansion.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Werner Engelmaier
Sent: Wednesday, February 03, 2010 8:13 AM
To: [log in to unmask]
Subject: Re: [TN] track lifting
Hi Brian,
I would appreciate pictures, possibly also to Steve, that I could use in my
reliability column—this is a failure mode fairly new and unknown to most
people.
If you could, I also would appreciate the base material, the peak reflow
temperature, the cooling rate after reflow, the Cu trace thickness and whether
it was covered with solder, and what solder. I now, its asking a lot, but only
with all the pertinent info can we make sense of this.
Werner
-----Original Message-----
From: Brian Chandler <[log in to unmask]>
To: [log in to unmask]
Sent: Wed, Feb 3, 2010 7:28 am
Subject: Re: [TN] track lifting
We just conducted a study on acceptable strain levels for lead free products.
Our BGA test coupons showed this exact result from excess strain.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
-------------------------------------------------------------------------------Leadfee Mail List provided as a service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Leadfree
To temporarily stop/(start) delivery of Leadree for vacation breaks send: SET Leadfree NOMAIL/(MAIL)
Search previous postings at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-------------------------------------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|