Hi Ioan! I have conducted a number of leadfree soldering investigations
with SAC405 and SAC305 solder paste using Immersion silver pwbs in
accordance with the IPC-4553 specification and have had no issues. The
higher leadfree processing temperatures tend to degrade all printed wiring
board surface finishes a bit faster than in tin/lead processing. I
recommend you investigate to see if the Immersion silver meets the IPC
4553 requirements.
Dave Hillman
Rockwell Collins
[log in to unmask]
Ioan Tempea <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
02/15/2010 10:06 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
Ioan Tempea <[log in to unmask]>
To
[log in to unmask]
cc
Subject
[TN] Lead-free soldering on ImAg
Dear Technos,
I know the ImAg has been discussed over and over and with the same
results, very good and reliable finish.
My little something now is all the proponents were mainly in high-rel
applications (so SnPb solder most likely) and I do not remember if RoHS on
Ag was discussed. I know it wouldn't make sense for this finish not to
work with SAC305 pastes, but I just want to make sure.
We have, guess what, wetting issues on two different boards, from the
same supplier. We have tried playing with the reflow recipe, no
improvement. The batch finished, but now we are attacking a few more
different models
from the same PCB fab.
So, did anybody have issues with ImAg because they were on lead-free? Any
particular parameters that are not a happy ingredient, like specific types
of paste, specific solder recipe milestones?
If it were the PCBs, what could be wrong except for the Ag thickness? I
mean XRF analysis would be cheaper than x-sectioning...
Thanks,
Ioan Tempea, ing.
Ingénieur Principal de Fabrication / Senior Manufacturing Engineer
T | 450.967.7100 ext.244
E | [log in to unmask] <mailto:[log in to unmask]>
W | www.digico.cc <http://www.digico.cc/>
N'imprimer que si nécessaire - Print only if you must
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|