Hi Steve - you are correct, there are three basic definitions have been
established to keep soldering, brazing and welding from becoming confused
terms:
Soldering - the joining of two metals by heating them to a suitable
temperature below their solidus and applying a filler metal having a
liquidus temperature below 450C
Brazing - the joining of two metals by heating them to a suitable
temperature below their solidus and applying a filler metal having a
liquidus temperature above 450C
Welding - the joining of two metals by heat or pressure, with or without a
filler metal, to produce a localized union through fusion
Sometimes folks use brazing and soldering interchangeably.
Dave
Steven Creswick <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
02/11/2010 07:06 PM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
Steven Creswick <[log in to unmask]>
To
[log in to unmask]
cc
Subject
Re: [TN] Old reference for silver solder - what's it cross ref to?
Graham,
I thought I would have an earlier version as well, but alas I do not.
In any case, my recollection was that this spec was for the more generic
'solders' [at <300-400°C liquidus] and not the more higher temp 'brazes'
like the 780°C CuAg eutectic.
My use of the terms 'solders' and 'brazes' may not be totally correct
[Dave
H can provide clarification], but I would suggest, as others have, that
the
'silver' solder you are looking for is the low temp Sn62 Pb36 Ag2 [Sn62 at
180°C], or Sn96.3 Ag 3.7 [which we used to call 'Sn96/4' or Sn96 at
221°C],
both being eutectic solders.
We used to use both for soldering on thick film Ag, Pd/Ag, or Pt/Pd/Ag's
to
mitigate leaching of the Ag bearing inks.
Since this is apparently for a PWB application, I think one could
reasonably
argue that anything above Sn96/4 is unlikely to be desired.
Get snow?! Michigan dug out again. Will let you know how the next round
is..
Steve C
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|