Hi Chris - with the proper equipment setup and calibration standards, XRF
can measure a Ni/Pd/Au plating stackup.
Dave Hillman
Rockwell Collins
[log in to unmask]
Chris Mahanna <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
01/21/2010 08:51 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
Chris Mahanna <[log in to unmask]>
To
[log in to unmask]
cc
Subject
Re: [TN] NiPdGold Plating Soldering Issues
Mumtaz,
Note that the Ni skips are on the tensile side of the lead only, not the
compression side. The lead was formed after finish plating, and the Ni
was pulled apart (Pd and Au too). It looks like it is breaking at the
thin spots caused by the surface of the lead?
This is a common cause of poor wetting.
Vlad,
There is a little debate within 6012/2221/455X now about quality assurance
of ENEPIG for wire bonding. The idea would be for the Au to be on the
thickness high-end of what's possible. 6012C weasel worded it. 2221B
pointed to pull testing. As I understand it, 455X is leaning towards XRF.
I don't personally know of a capable XRF/ standard. Any ideas? I
suggested that maybe FIB mill + SEM might work better and be more
available than $150k XRFs, but I haven't tried it.
Chris
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Mumtaz Bora
Sent: Wednesday, January 13, 2010 5:28 PM
To: [log in to unmask]
Subject: Re: [TN] NiPdGold Plating Soldering Issues
Hello Vladimir,
The Nickel plating thickness was measured using SEM. Palldium and Gold
were measured using XRF.
Mumtaz Bora
Senior Quality Engineer
Peregrine Semiconductor
9380 Carroll Park Drive
San Diego, CA 92121
858-795-0112-direct
858-731-9499 -fax
[log in to unmask]
SMTAI, October 6-7, 2009 in San Diego, CA - a world-class conference and
exhibition devoted to electronics assembly. Visit www.smta.org/smtai for
full details.
For a free exhibit pass:
http://smta.org/smtai/Free_Exhibits_Pass_SMTAI.pdf
-----Original Message-----
From: vladimir Igoshev [mailto:[log in to unmask]]
Sent: Wednesday, January 13, 2010 1:10 PM
To: TechNet E-Mail Forum; Mumtaz Bora
Subject: Re: [TN] NiPdGold Plating Soldering Issues
Mumtaz,
One can not measure such thin layers (Au in particular) with SEM, unless
the sample was specially prepared (overplated with Ni). Did you do that?
Regards,
Vladimir
SENTEC
11 Canadian Road, Unit 7.
Scarborough, ON M1R 5G1
Tel: (416) 899-1882
Fax: (905) 882-8812
www.sentec.ca
-----Original Message-----
From: Mumtaz Bora <[log in to unmask]>
Date: Wed, 13 Jan 2010 12:07:49
To: <[log in to unmask]>
Subject: Re: [TN] NiPdGold Plating Soldering Issues
Hi Victor,
Yes, I have SEM/EDX images of the component. SEM was used for plating
thickness measurements . Base material is copper. No idea on the dwell
time from Nickel to Gold.
Mumtaz Bora
Senior Quality Engineer
Peregrine Semiconductor
9380 Carroll Park Drive
San Diego, CA 92121
858-795-0112-direct
858-731-9499 -fax
[log in to unmask]
SMTAI, October 6-7, 2009 in San Diego, CA - a world-class conference and
exhibition devoted to electronics assembly. Visit www.smta.org/smtai for
full details.
For a free exhibit pass:
http://smta.org/smtai/Free_Exhibits_Pass_SMTAI.pdf
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Victor Hernandez
Sent: Wednesday, January 13, 2010 6:49 AM
To: [log in to unmask]
Subject: Re: [TN] NiPdGold Plating Soldering Issues
Do you have SEM/EDX photos of this sample/cross section?
What instrument was used to measure the plating? XRF or SEM What is base
material?
Dwell time from nickel to Au plating?
Vic,
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Steve Gregory
Sent: Tuesday, January 12, 2010 6:23 PM
To: [log in to unmask]
Subject: Re: [TN] NiPdGold Plating Soldering Issues
Hi Mumtaz!
It's been a long while since anybody has asked me to post anything on my
webpage, TechNet has been pretty quiet for the last couple of months. I
have been pretty quiet myself for awhile. I've had a lot of changes in my
life recently.
Anyways, I have your PowerPoint posted, it's here:
http://stevezeva.homestead.com/Mumtaz.ppt
Sure looks like "head-in-pillow" to me.
Hope you have a good 2010.
Kind regards,
Steve Gregory
--- [log in to unmask] wrote:
From: Mumtaz Bora <[log in to unmask]>
To: [log in to unmask]
Subject: [TN] NiPdGold Plating Soldering Issues
Date: Tue, 12 Jan 2010 14:56:12 -0800
Hello Technetters,
We have some SC70 packages with NiPd gold plating that have wetting issues
.
Customer is using Kester R596L tinlead water soluble solder paste
conducting eutectic reflow at 227C peak and have wetting issues.(first
3 images in PowerPoint).
We have checked plating thickness with our supplier and it meets spec.
EDX did not show any contamination, oxides etc. JEDEC solderability test
passed.
X-section shows some areas of missing nickel or gaps in coverage of base
copper. I need the experts to look at the images and comment if this could
be the root cause of poor wetting and non-wetting.
I have forwarded the PowerPoint to Steven Gregory to post on his website.
Your feedback will be much appreciated.
Thank-you
Mumtaz Bora
Senior Quality Engineer
Peregrine Semiconductor
9380 Carroll Park Drive
San Diego, CA 92121
858-795-0112-direct
858-731-9499 -fax
[log in to unmask]
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts:
send e-mail to [log in to unmask]: SET Technet Digest Search the archives of
previous posts at: http://listserv.ipc.org/archives Please visit IPC web
site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|