TECHNET Archives

January 2010

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>
Date:
Tue, 19 Jan 2010 13:49:08 -0500
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Chris Mahanna <[log in to unmask]>
Subject:
From:
Chris Mahanna <[log in to unmask]>
MIME-Version:
1.0
In-Reply-To:
Content-Transfer-Encoding:
quoted-printable
Content-Type:
text/plain; charset="us-ascii"
Parts/Attachments:
text/plain (93 lines)
Werner, Vlad, Paul-
Thanks for reassuring me that we are playing the probabilities correctly.  We've used sectioning/lapping, polarizer/analyzer, and SEM/EDS (to find the Cu, Br) successfully many times.  Our problem this time is that we need to grow one.  We used four of the actual boards, with 12 opportunities each = 48 total.  A good CAF test vehicle would have 100s.  We used 2 cycles of 2.6.27 260C profile for precondition.   Customer wanted 2 cycles and actual product bias voltage (3.3V), which doesn't help us accelerate.  Oh well.  I was just wondering if anyone would reply "hey those MSPs will short if they were damaged..."

Chris

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of vladimir Igoshev
Sent: Tuesday, January 19, 2010 11:43 AM
To: [log in to unmask]
Subject: Re: [TN] TI MSP Early Life Failure?

Chris,

Werner is right, it's difficult, yet doable to prove you are dealing with CAF. You'd need to have sectionning, as well as lapping done to find Cu between fibers and resin in the board.

Regards,

Vladimir
SENTEC
SENTEC
11 Canadian Road, Unit 7.
Scarborough, ON M1R 5G1
Tel: (416) 899-1882
Fax: (905) 882-8812
www.sentec.ca

-----Original Message-----
From: Werner Engelmaier <[log in to unmask]>
Date:         Tue, 19 Jan 2010 11:25:37 
To: <[log in to unmask]>
Subject: Re: [TN] TI MSP Early Life Failure?

 Hi Chris,
Your scenario sure points towards CAF given the reflows, the via spacing, the timing of the failures, the high resistance of the shorts.
And yes, 'proving' CAF is difficult at best. What are you trying to do to 'prove' CAF?
IMHO, the best you can do is finding circumstantial evidence--the best is rough drilled hole walls on other vias with Cu-plating along separations of glassfibers and resin.
Werner

 


 

 

-----Original Message-----
From: Chris Mahanna <[log in to unmask]>
To: [log in to unmask]
Sent: Tue, Jan 19, 2010 11:13 am
Subject: [TN] TI MSP Early Life Failure?


Hello Technet,
We are working on a failure analysis of a battery operated remote sensing device.  Failure is linked to 500ohm short power/ground.  The assembly experiences at least (2) 255C reflow thermal excursions.  Failure manifests at
~6 months.
Slicing/dicing isolation yielded: breakdown between two vias (17 mil spacing) and/or MSP input impedance.  Beyond that, original evidence is lost.
We are working the CAF theory, however reproduction of the problem is proving difficult, possibly due to the low number of opportunities on the actual board.
For those of you who know that I'm pushing for placement of (the new) CAF coupons on panels, yes this is our most recent example of the problem.

I would like to get feedback on the possibility that it was the microcontroller instead...

TI MSP430F1612
Level-3-260C-168 HR


Thanks!

Chris Mahanna
Robisan Laboratory Inc.

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

 

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2