It all boil down to volume vs price. If you have volume and price advantage, you will find the top supply house (at least one or two, if not three). No standard required. It is such a highly specialized area that in house spec is good enough. The guys make the high end large volume even has wire bonder in QA with the bond pull force listed for every batch (if you pay top dollar).
--------------------------
Sent using BlackBerry
----- Original Message -----
From: TechNet <[log in to unmask]>
To: [log in to unmask] <[log in to unmask]>
Sent: Wed Jan 06 09:17:55 2010
Subject: Re: [TN] Pull strength of thermosonic wire bondable gold
This begs the question, are there IPC or other standards for die and wire bonding that define what the specific alloys and nickel thickness and the gold thickness ranges shall be, similar to those within IPC 4552 and 4553?
Looking back at these issues in doing a search of the forum archives, it appears that this is an issue that many people keep struggling with.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of [log in to unmask]
Sent: Wednesday, January 06, 2010 8:14 AM
To: [log in to unmask]
Subject: Re: [TN] Pull strength of thermosonic wire bondable gold
Hi Steve,
Nickel below 80-90 microinches will not act as a barrier due to porosity. You may get copper migration at 40 microinches of Ni which will effect bonding.
Regards
Aleks Lozinsky
Technical Sales Representative
Technic Canada Inc.
Office: 905-940-4020
Cell: 416-450-1093
E-mail: [log in to unmask]
-----Original Message-----
From: Steve Kelly <[log in to unmask]>
Date: Wed, 6 Jan 2010 08:50:49
To: <[log in to unmask]>
Subject: Re: [TN] Pull strength of thermosonic wire bondable gold
Hi Steve et al,
Unfortunately this is not as easy as it sounds. First the lower pull
strengths are not necessarily a failure- they are just not as good. This was
an experiment designed between ourselves and our customer. The initial
problem is we have a .0032 wide flying lead ( about 150 of them) with no
kapton support. A chip/die is "compression bonded" onto the lead - from what
I can gather it is a combination of heat/pressure/ultrasonic and some kind
of proprietary magic. The reason we went to the lower nickel is because the
leads being so fragile they often crack during the process so we tried the
lower nickel to alleviate this issue. With the lower nickel pull is approx.
5-7 grams. With the higher nickel 9-11 grams. There is a gold bump on the
die and when the failure happens the gold bump separates from the lead with
no damage to the gold bump. At present this is as much as I know. Thanks for
the input so far. Steve Kelly
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Steven Creswick
Sent: January-05-10 6:14 PM
To: [log in to unmask]
Subject: Re: [TN] Pull strength of thermosonic wire bondable gold
Steve,
If you can send me the data sets in an Excel format, I can provide you with
some insight based on magnitude and grouping by Weibull plot.
If there is a big mix of failure modes, this interpretation will be pretty
generic.
Its free input, however :-)
Just send it direct.
Steve C
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Steve Kelly
Sent: Tuesday, January 05, 2010 4:17 PM
To: [log in to unmask]
Subject: [TN] Pull strength of thermosonic wire bondable gold
Hi All,
I have a wire bond question to the wire bond gurus who have helped me out a
lot in the past. Made 2 versions of a flex circuit - only varied the nickel
thickness. Application is thermosonic gold wire bonding.
Flex circuit lead is .0032 wide - version 1 - nickel is 150 microinches -
soft gold is 50 microinches- pull strength is X
Version 2 - nickel
is 40 microinches - soft gold is 50 microinches - pull strength is approx.
½X of version 1-
Is this what I should expect?
Regards Steve Kelly
Steve Kelly (PLEASE NOTE NEW E-MAIL ADDRESS)
(416) 750-8433 (work)
(416) 750-0016 (fax)
(416) 577-8433 (cell)
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|