TECHNET Archives

November 2009

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, Bev Christian <[log in to unmask]>
Date:
Sat, 7 Nov 2009 16:36:28 +0000
Reply-To:
Subject:
From:
Vladimir Igoshev <[log in to unmask]>
MIME-Version:
1.0
In-Reply-To:
Content-Type:
text/plain; charset="Windows-1252"
Content-Transfer-Encoding:
base64
Parts/Attachments:
text/plain (1 lines)
Bev,



I'm not that much sure about the definition of the "voids...  open to the surface" and how they may affect the reliability.  Remember, that voids do next to nothing in terms of stress concentration.



Regards,



Vladimir

SENTEC

11 Canadian Road, Unit 7.

Scarborough, ON M1R 5G1

Tel: (416) 899-1882

Fax: (905) 882-8812

www.sentec.ca





-----Original Message-----

From: Bev Christian <[log in to unmask]>

Date:         Sat, 7 Nov 2009 11:10:50 

To: <[log in to unmask]>

Subject: Re: [TN] Solder Voids in Chip Components



Correct. Or the voids are open to the surface, as Joyce K pointed out to me. 

Bev



----- Original Message -----

From: TechNet <[log in to unmask]>

To: [log in to unmask] <[log in to unmask]>

Sent: Sat Nov 07 11:02:58 2009

Subject: Re: [TN] Solder Voids in Chip Components



Unless there is a significant "segregation" of rather small voids at one of the interfaces :-)



Vladimir

SENTEC

11 Canadian Road, Unit 7.

Scarborough, ON M1R 5G1

Tel: (416) 899-1882

Fax: (905) 882-8812

www.sentec.ca





-----Original Message-----

From: Bev Christian <[log in to unmask]>

Date:         Sat, 7 Nov 2009 10:59:31 

To: <[log in to unmask]>

Subject: Re: [TN] Solder Voids in Chip Components



Alejandro,

No there is not. 



In the 10 years I was at Nortel we could never see any significant difference between shear strength of solder joints with low voiding and those that looked like Swiss cheese (up to 50% voiding). I am sure that Werner will come back and rightly say that shear strength does not necessarily equate to solder joint reliability. But I can say we never saw chip cap problems that were traceable to the joint voids. 

Bev



----- Original Message -----

From: TechNet <[log in to unmask]>

To: [log in to unmask] <[log in to unmask]>

Sent: Sat Nov 07 10:40:25 2009

Subject: [TN] Solder Voids in Chip Components



Hello,



Does anybody know if there is an IPC specification that describes the amount of solder voids allowed in a chip component solder joint?  The IPC-A-610 Rev D is specific describing the % of voids allowed for BGA's solder joints (<25%) only but not for any other type of components.     



Saludos Cordiales / Best Regards 

Alejandro A. Domínguez 

Robert Bosch Corporation







---------------------------------------------------

Technet Mail List provided as a service by IPC using LISTSERV 15.0

To unsubscribe, send a message to [log in to unmask] with following text in

the BODY (NOT the subject field): SIGNOFF Technet

To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)

To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest

Search the archives of previous posts at: http://listserv.ipc.org/archives

Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815

-----------------------------------------------------



---------------------------------------------------------------------

This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful.



---------------------------------------------------

Technet Mail List provided as a service by IPC using LISTSERV 15.0

To unsubscribe, send a message to [log in to unmask] with following text in

the BODY (NOT the subject field): SIGNOFF Technet

To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)

To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest

Search the archives of previous posts at: http://listserv.ipc.org/archives

Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815

-----------------------------------------------------





---------------------------------------------------------------------

This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful.



---------------------------------------------------

Technet Mail List provided as a service by IPC using LISTSERV 15.0

To unsubscribe, send a message to [log in to unmask] with following text in

the BODY (NOT the subject field): SIGNOFF Technet

To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)

To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest

Search the archives of previous posts at: http://listserv.ipc.org/archives

Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815

-----------------------------------------------------




ATOM RSS1 RSS2