Rex,
I would check the BGA ball composition as your problem may come from a
head-in-pillow effect.
Low-Ag SAC BGAs are becoming more and more common and BGA ball
composition is often not well specified (SAC is now a wide family...).
Low-Ag SAC ball composition may be the reason to call for higher reflow
temperatures.
I have had the information (but not checked) that ATMEL AT91SAM9G20-CU
(which looks close to your reference and has the same LFBGA217 package)
has SAC105 balls.
Rex Waygood a écrit :
> We have built a batch of pcbs for a customer who supplied the pcbs. They
> are 2mm thick 6 layer with 0.2mm vias and ENIG finish. None work fully,
> they work intermittently at best.
>
> The customer was suspicious that we had not reflowed the BGAs correctly.
>
> Our under BGA temp on a similar pcb is 245C (We now have some samples to
> profile correctly)
>
> The customer is suspicious due to the comment on page 753
> http://www.atmel.com/dyn/resources/prod_documents/doc6221.pdf
> <http://www.atmel.com/dyn/resources/prod_documents/doc6221.pdf> where
> it states a min of 250C
>
> Close x-ray evaluation of the BGAs showed tear dropping along tracks,
> uniform balls, everything looked tickety boo.
>
> We offered to remove a BGA to see what was happening underneath.
>
> 2 corners showed a similar issue with the ball where it separated from
> the BGA rather than the pcb.
>
> The removal technique was to use a PDR IR rework station, under board
> heating to bring topside pcb temp to 170C and then a lead free reflow
> profile to bring the device up to reflow, manual removal.
>
> I didn't have dye for dye and pry so thought this might show if there
> was an ENIG problem.
>
> I was surprised by the almost complete removal of ball at the device and
> lack of evidence of solder.
>
> Was this just caused by my investigation processes?
>
> Was the ball device interface broken which prevented it from melting the
> ball?
>
> Any other clues?
>
> Thanks
>
> Rex
>
>
>
> Hopefully Steve has received the images (sorry about the size!)
>
>
> Rex Waygood
> Technical Manager
>
> Hansatech EMS provides value manufacturing through engineering and
> quality
>
> ________________________________
>
>
> Hansatech EMS Limited
> Benson Road
> Nuffield Industrial Estate
> Poole
> Dorset BH17 0RY
> United Kingdom
>
>
> Tel:
> Fax:
> DDI: +44 (0)1202 338200
> +44 (0)1202 338202
> +44 (0)1202 338222
> [log in to unmask]
> www.HansatechEMS.com <http://www.hansatechems.com/>
>
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
> -----------------------------------------------------
>
--
Arnaud Grivon
Thales Corporate Services - EPM
18, Avenue du Maréchal Juin
Bât. C - Bureau C2-135
92366 MEUDON LA FORET Cedex
Tél : (+33) (0)1 70 28 23 88
"The information contained in this e-mail/fax and any attachments are the property of THALES and may be confidential. If you are not the intended recipient, please notify us immediately, send this message back to us and destroy it. You are hereby notified that any review, dissemination, distribution, copying or otherwise use of this e-mail/fax is strictly prohibited."
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|