TECHNET Archives

November 2009

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
Date:
Tue, 17 Nov 2009 20:49:00 +0100
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Inge <[log in to unmask]>
Subject:
MIME-Version:
1.0
Content-Transfer-Encoding:
quoted-printable
Content-Type:
text/plain; charset="iso-8859-1"
From:
Parts/Attachments:
text/plain (105 lines)
Hi W,

Es war nicht zu beleidigen, just played with white paper ...
Inge



  ----- Original Message ----- 
  From: Werner Engelmaier 
  To: [log in to unmask] ; [log in to unmask] 
  Sent: Tuesday, November 17, 2009 4:58 PM
  Subject: Re: [TN] Microvia reliability vs Lead free


  Hi Inge,
  Bucks are green.
  But you should know, nothing good is for nothing. 
  I take it, you work pro bono for Saab ;-)
  Werner





  -----Original Message-----
  From: Inge <[log in to unmask]>
  To: TechNet E-Mail Forum <[log in to unmask]>; Werner Engelmaier <[log in to unmask]>
  Sent: Mon, Nov 16, 2009 11:14 pm
  Subject: Re: [TN] Microvia reliability vs Lead free


  Sure,Werner, with black payment? 
  /Inge 
   
  ----- Original Message ----- From: "Werner Engelmaier" <[log in to unmask]> 
  To: <[log in to unmask]> 
  Sent: Monday, November 16, 2009 5:04 PM 
  Subject: Re: [TN] Microvia reliability vs Lead free 
   
  Hi Inge, 
  Certainly have. This is not new, and it is not very surprising. 
  You may be interested in my White Paper on how to design PCBs for reiability given Pb'free soldering. 
  Werner 
   
  -----Original Message----- 
  From: Hernefjord Ingemar <[log in to unmask]> 
  To: [log in to unmask] 
  Sent: Mon, Nov 16, 2009 3:22 pm 
  Subject: Re: [TN] Microvia reliability vs Lead free 
   
   
   
  any relationships are described, one of which is a Curtiss-Wright report. They 
  ave exposed identical boards to SnPb soldering/repair and compared with same 
  or SACs, and found a significant difference in time to failure. 
   
    1st thermal cycle to failure 
    As Received 6 x 230 Celcius 6 x 260 
  elcius 
  Mean 788 443 4 
   
  That is a dramatic change in via failures. We have seen some failures recently 
  n ordinary double sided FR-4 boards, which were exposed to several heat 
  xposures in conjunction with electrical testing. Far from 260 Celcius, think 
  nly 125 Celcius. If we got microvia issues with only 125 C, what if we use 260 
  (e.g. repeated repair)? 
  Has anyone seen any signs of via failure due to increased heat exposure in 
  ractice? 
   
  nge 
  -------------------------------------------------- 
  echnet Mail List provided as a service by IPC using LISTSERV 15.0 
  o unsubscribe, send a message to [log in to unmask] with following text in 
  he BODY (NOT the subject field): SIGNOFF Technet 
  o temporarily halt or (re-start) delivery of Technet send e-mail to 
  [log in to unmask]: SET Technet NOMAIL or (MAIL) 
  o receive ONE mailing per day of all the posts: send e-mail to 
  [log in to unmask]: SET Technet Digest 
  earch the archives of previous posts at: http://listserv.ipc.org/archives 
  lease visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for 
  dditional information, or contact Keach Sasamori at [log in to unmask] or 
  47-615-7100 ext.2815 
  ---------------------------------------------------- 
   
  --------------------------------------------------- 
  Technet Mail List provided as a service by IPC using LISTSERV 15.0 
  To unsubscribe, send a message to [log in to unmask] with following text in 
  the BODY (NOT the subject field): SIGNOFF Technet 
  To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) 
  To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest 
  Search the archives of previous posts at: http://listserv.ipc.org/archives 
  Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 
  ----------------------------------------------------- 
   

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2