Good decision. The one pin with excess solder confused me. I was about
to point out that all of the other pins that display the gray areas do
so with a very clean line of demarcation between the exposed
underplating and the gold. This indicates that it was some type of
plating issue at the connector vendor. It looks like some tape or
tooling was applied, and it affected the gold plating onto the basis
metal, which looks like nickel in the pictures.
These connectors should be removed and replaced with those from an
entirely different lot code that are pre-screened under 30X inspection
for any evidence of plating issues.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Justin Braime
Sent: Thursday, October 08, 2009 2:43 AM
To: [log in to unmask]
Subject: Re: [TN] gold connector discoloration
Thanks for your input guys.
The appearance of the connectors is fairly consistent across all the
PCBs in
the batch. So either there was some touching up done very consistently,
or
they've increased solder paste volume - the contractor uses the Mydata
'solder jet' technology rather than stencil printing.
Apart from one pin on that one PCB, there's no solder on the gold mating
surfaces, but the purple/black discoloration (it's not very clear on the
photos compared to the actual view through the stereo microscope)on
lower
parts of the mating surfaces is widespread - not sure if this is flux
wicking up the lead and causing the gold to tarnish, or even nickel
passivation following gold dissolution? Either way, I've got misgivings
about the reliability, so back the PCBs will go!
Many thanks,
Justin
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Paul Edwards
Sent: 07 October 2009 18:14
To: [log in to unmask]
Subject: Re: [TN] gold connector discoloration
I agree with Victor on the solder-on-Au-connector issue...
Looks to me that someone either reworked or touched-up the connectors
after
SMT or they hand soldered the connectors in...
Adding flux to the connector and touching the SJs to clear a solder
short or
(most likely) to add solder to the joint will cause solder to wet up
into
the contact area on low profile connectors...Extra heat starts it but
too
much solder and flux does it every time...
You'll have to ask the CM to remove and replace the connectors...
Paul
Paul Edwards
Surface Art Engineering
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Victor Hernandez
Sent: Wednesday, October 07, 2009 10:06 AM
To: [log in to unmask]
Subject: Re: [TN] gold connector discoloration
Beware of fretting with the solder on the gold plated contacts.
Victor,
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Gumpert, Ben
Sent: Wednesday, October 07, 2009 9:34 AM
To: [log in to unmask]
Subject: Re: [TN] gold connector discoloration
Justin,
It looks like you have some solder that has made its way up the gold.
The picture of the prior board looked as if there was less solder used
to attach the connector, as there is still evidence of gold on the leads
(where solder has not covered the leads as it has done in the 'new
batch' image).
Maybe they installed connectors that had been tinned, so there was
additional solder in the process.
Ben
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Justin Braime
Sent: Wednesday, October 07, 2009 10:12 AM
To: [log in to unmask]
Subject: [TN] gold connector discoloration
Hi Technetters,
We've just received a new batch of boards from one of our
subcontractors,
and the Hirose DF12 header sockets have discoloration on the mating
terminals.
On previous batches, we have seen a little discoloration adjacent to the
solder joints, but never up in the connector mating area itself. The
process
hasn't (allegedly) changed.
I've posted some pics at:
http://gallery.me.com/jbraime/100005
Any ideas as to the cause? Any detriment to functionality?
Thanks in advance,
Justin
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please visit http://www.messagelabs.com/email
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|