Hi Vladimir,
Maybe we should simply drop the name 'Black Pad' entirely—too much baggage and confusion.
Maybe we should refer to them by their failure modes and damage mechanisms—solderability issues due to 'galvanic corrosion', brittle fracture due to P-enrichment, brittle fracture due to 'any other cause applicable.
Werner
-----Original Message-----
From: [log in to unmask]
To: Werner Engelmaier <[log in to unmask]>; [log in to unmask]
Sent: Wed, Oct 21, 2009 7:39 am
Subject: Re: [TN] ENIG Issue
Werner,
Yes, I agree that there are two different phenomena BP and BF, but I can not agree on the statement that the root cause for BF(brittle fracture) is high P content.
Regards,
Vladimir
SENTEC
11 Canadian Road, Unit 7.
Scarborough, ON M1R 5G1
Tel: (416) 899-1882
Fax: (905) 882-8812
www.sentec.ca
From: Werner Engelmaier <[log in to unmask]>
Date: Tue, 20 Oct 2009 23:59:34 -0400
To: <[log in to unmask]>; <[log in to unmask]>
Subject: Re: [TN] ENIG Issue
Vladimir,
Indeed you sent me that ATOTECH paper, but I have several references that disagree with their definition, as well as others that agree with the Atotech paper.
There seem to be (at least) 2 different 'defects' at work—one with hyper-galvanic corrosion of the Ni during Au-plating causing soldering problems, and another causing brittle separation due to a weakened interface cause by too much P.
Are we in agreement on this?
I do not really care what you call either of them—clearly the root cause is different in these cases and so is what needs to be done.
Clearly, what we need is for the IPC to form a committee to provide proper definitions and 'names.'
Werner
-----Original Message-----
From: [log in to unmask]
To: TechNet E-Mail Forum <[log in to unmask]>; Werner Engelmaier <[log in to unmask]>
Sent: Tue, Oct 20, 2009 11:23 pm
Subject: Re: [TN] ENIG Issue
Werner,
We've been through it several times already. As far as I know, BP was defined as
a case of poor Ni-P plating with cavitation present in the layer. I think I sent
you an old ATOTECH paper on the topic a while ago.
Regards,
Vladimir
SENTEC
11 Canadian Road, Unit 7.
Scarborough, ON M1R 5G1
Tel: (416) 899-1882
Fax: (905) 882-8812
www.sentec.ca
-----Original Message-----
From: Werner Engelmaier <[log in to unmask]>
Date: Tue, 20 Oct 2009 22:57:21
To: <[log in to unmask]>
Subject: Re: [TN] ENIG Issue
Hi Vladimir,
Then we are not communicating.
Please explain to me what YOU mean by 'BP failure'.
When I say 'BP failure', I mean it is because too much P between the Ni and the
IMC layers has weakened the bond leading to brittle separation on sufficient
loading. I do not differentiate as to the cause(s) for too much P. For me they
describe a damage mechanism.
You can similar appearance with too much and too little P.
Werner
-----Original Message-----
From: [log in to unmask]
To: Werner Engelmaier <[log in to unmask]>; [log in to unmask]
Sent: Tue, Oct 20, 2009 10:44 pm
Subject: Re: [TN] ENIG Issue
Werner,
You just confirmed what I said in my previous e-mail. You customer got failure
with black appeared pads, but it wasn't BP failure. Similar appearance doesn't
mean the same mechanism.
Regards,
Vladimir
SENTEC
11 Canadian Road, Unit 7.
Scarborough, ON M1R 5G1
Tel: (416) 899-1882
Fax: (905) 882-8812
www.sentec.ca
From: Werner Engelmaier <[log in to unmask]>
Date: Tue, 20 Oct 2009 22:16:40 -0400
To: <[log in to unmask]>; <[log in to unmask]>
Subject: Re: [TN] ENIG Issue
Hi Vladimir,
I have one client who experienced 'Black Pad' after 9(!) soldering operations.
The P-content got progressively worse; it peaked with the EDS spikes for P being
as high as those for Sn.
Werner
-----Original Message-----
From: [log in to unmask]
To: TechNet E-Mail Forum <[log in to unmask]>; Werner Engelmaier
<[log in to unmask]>
Sent: Tue, Oct 20, 2009 10:07 pm
Subject: Re: [TN] ENIG Issue
Werner,
With all due respect, I don't think you are right.
Regards,
Vladimir
SENTEC
11 Canadian Road, Unit 7.
Scarborough, ON M1R 5G1
Tel: (416) 899-1882
Fax: (905) 882-8812
www.sentec.ca
-----Original Message-----
From: Werner Engelmaier <[log in to unmask]>
Date: Tue, 20 Oct 2009 22:01:35
To: <[log in to unmask]>
Subject: Re: [TN] ENIG Issue
Hi George,
\While what you say in the first paragraph is correct, the second paragraph is
not.
'Black Pad' is not an all-or-nothing proposition. The seeds are sown at the
Ni-plating (not the Au-plating) with the P-codeposition. However, multiple or
lengthy expositions to high soldering temperatures result in more Ni being
dissolved to form IMCs leaving ever more P behind. This can create 'Black Pad'
where none existed before.
Werner
-----Original Message-----
From: George Milad <[log in to unmask]>
To: [log in to unmask]
Sent: Tue, Oct 20, 2009 9:52 pm
Subject: Re: [TN] ENIG Issue
As always as soon as there is a solderability issue with ENIG, "Black pad"
comes up. This is a problem because it does not allow for further
investigation. Everyone accepts since this is ENIG then it must be black pad.
If this was a black pad issue the back side should have exhibited the same
problem. BP occurs during the plating of the gold on top of the Ni. BP
cannot differentiate one side from the other.
Do not accept BP as the answer and keep investigating.
Regards
George Milad
George Milad
National Accounts Manager for Technology
Uyemura International Corp (UIC)
249 Town Line Rd
Southington CT 06489
[log in to unmask]
Cell: (516) 901 3874
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|