10 mils (0.25mm) via in pad is too big diameter for this (main reason for voids), why not laser drilling.
Best Regards
Reuven ROKAH
Think green before printing this mail... Thanks
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Douglas McCall
Sent: Tuesday, October 13, 2009 1:07 PM
To: [log in to unmask]
Subject: [TN] BGA voids in filled & capped micro-via PWB
Hi,
We have non-conductive resin filled and capped micro-via (via-in-pad) through the complete PWB thickness (1.6mm FR4) 8-layer, we have seen considerable voiding in the BGA balls following assembly:
Q1) What is the chance of out-gassing from the PWB board (or specifically the filled capped via) going into the BGA ball and creating a void during reflow.
Q2) What is adequate flatness on the PWB surface considering “dish-down” of the filled resin during via filling and before Cu plating. I think the IPC spec. is 70% but does anyone have differing experience of this.
Q3) Would a fairly “rough” topology on the surface of the capping plating (i.e. not totally flat, bumps etc) cause any difference in the solderability,
I believe that:
· The via drilled diameter is 0.25mm
· PWB finish ENIG,
· Cu/Ni/Au plating thickness is 20um
· The PWB thickness is 1.6mm
· The PWB Tg is approx 170 deg-C
· The paste is Pb-free,
· The reflow profile is good to the paste suppliers recommended profile,
· The PWB’s have been baked-out 130 deg-c 24-hours before assembly,
· Reflow peak reached 242 deg-C
· Reflow soak 170 deg-C for 170 seconds,
There are large and small voids in the BGA balls during X-Ray and cross sectioning. Some of the BGA balls apear slightly elongated not correct shape.
In essence would you think that it would be a PWB issue or assembly problem.
Any feedback would be much appreciated.
Thanks,
D. McCall.
mailto: [log in to unmask]
_________________________________________________________________
Save time by using Hotmail to access your other email accounts.
http://clk.atdmt.com/UKM/go/167688463/direct/01/
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|