Hello Jim,
As a solder mask service bureau we will apply a double coat of solder mask
to customer products that have high copper plating requirements. In most
cases there is a high power requirement and the customer cannot take a
change of having a pin hole in the solder mask which could arch to a
component or ground.
You did not mention in your e-mail if the solder mask was a liquid or a dry
film solder mask. I am guessing it is a liquid solder mask.
It is possible that your supplier saw some exposed copper after applying the
first coat of Liquid Photoimageable Solder Mask (LPISM) due to the 2 oz of
copper. The supplier may have decided to apply a second coat to insure
coverage.
Possible you may want to consider a Mixed Technology coating. Dry Film
Solder Mask (DFSM) and Liquid Photoimageable Solder Mask. Of course this
will increase your board cost but may be better for you product in the long
run.
While bubbles can be created between the layers of mask it is not something
that I would accept.
Regarding the stringers of solder mask across pads. This is not acceptable.
Regards,
Frank Kurisu
SolderMask, Inc.
714 842-1987 - Office
714 454-0539 - Mobile
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of James Mahoney
Sent: Thursday, October 29, 2009 5:48 AM
To: [log in to unmask]
Subject: Re: [TN] Bare Board Quality (mask issues)
We would only use the double process for thick copper weights. Sounds like a
rework that didn't go very well.
www.quickturnflex.com
Thank you,
Jim Mahoney
Quick Turn Flex Circuits, LLC
Applications Project Manager
P# 603-821-7071
M# 603-305-6250
P Please consider the environment before printing this e-mail
** This email and all attachments have been scanned prior to being sent**
Confidentiality Notice: This page and any accompanying documents contain
information that is confidential, privileged or exempt from disclosure and
is intended for the exclusive use of the addressee. If you are not the
intended recipient, you are hereby notified that any disclosure, copying,
distribution or use of the contents of this information in any manner is
strictly prohibited.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of J W
Sent: Thursday, October 29, 2009 8:41 AM
To: [log in to unmask]
Subject: [TN] Bare Board Quality (mask issues)
Hi,
Looking for some expertise regarding bare board fabrication and the solder
mask process. We have a supplier (China) that decided to add two layers of
mask versus one layer (not called out in our specifications). The reason
for doing this is explained by them below. Our end customer does not like
the two-layer mask and thought it was due to a rework process. I am not
familiar with a two-layer solder mask process, is this something new? Is
this OK? Their solution is to not do it anymore, but I want to understand
is this something others have seen and approved. If so, why?
In addition, during this two layer process, they say they will have air
bubbles (note 2 below), which we found in a cross section. They wrote that
going to one-layer would eliminate the air bubbles? Not sure if that is true
or if their process is questionable.
Lastly, we also found thin solder mask stringers stretched across some pads.
They claim dirty worktable (note 3 below) I wonder if this was caused by the
extra solder mask layer application?
I appreciate any comments.
Thanks,
Jim
*
COMMENTS FROM SUPPLIER
A1: (1) Supplier adopted twice solder mask coating process to produce this
PCB. They are NOT reworked PCB. As the copper thickness of this PCB is 2OZ ,
Supplier adopted twice solder mask coating process based on below
conception.
a: Considering the working power will be huge when PCBA's working, to
perform twice solder mask coating process will enhance PCB quality and
prolong PCB cycle life, preventing solder mask being broken down if the
solder mask aging after long time usage
b: As usage frequency of this PCB is higher than general PCB, adopting twice
solder mask coating process will prevent outside signal interferer for PCB
when the solder mask's aging.
(2) As adopt twice solder mask coating process, solder mask is too
thick(within 60~70um), the air bubbles in the solder mask is difficult to
get away
(3) The stringers on pad is caused by adhering foreign stuff from worktable
before OSP process."*
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet
NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send
e-mail to [log in to unmask]: SET Technet Digest Search the archives of
previous posts at: http://listserv.ipc.org/archives Please visit IPC web
site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet
NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send
e-mail to [log in to unmask]: SET Technet Digest Search the archives of
previous posts at: http://listserv.ipc.org/archives Please visit IPC web
site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|