TECHNET Archives

October 2009

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
Joyce Koo <[log in to unmask]>
Date:
Fri, 23 Oct 2009 11:42:56 -0500
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Subject:
From:
"David D. Hillman" <[log in to unmask]>
X-cc:
In-Reply-To:
Content-Type:
text/plain; charset="US-ASCII"
MIME-Version:
1.0
Parts/Attachments:
text/plain (3314 lines)
 It should be on the IPC 7093 committee page under drafts

Dave



"Joyce Koo" <[log in to unmask]> 
10/23/2009 11:30 AM

To
<[log in to unmask]>, <[log in to unmask]>
cc

Subject
Re: [TN] [spam] RE: [TN] ENIG Issue






Is any possibility just get the B?
--------------------------
Sent using BlackBerry


----- Original Message -----
From: TechNet <[log in to unmask]>
To: [log in to unmask] <[log in to unmask]>
Sent: Fri Oct 23 12:24:48 2009
Subject: Re: [TN] [spam] RE: [TN] ENIG Issue

The latest committee draft that just went out has Appendix B in it.

Dave



Werner Engelmaier <[log in to unmask]> 
10/23/2009 11:14 AM

To
[log in to unmask], [log in to unmask]
cc

Subject
Re: [TN] [spam] RE: [TN] ENIG Issue






Thanks Dave, 
my copy of 7093WD for some reason did not contain appendix B.
Werner


-----Original Message-----
From: David D. Hillman <[log in to unmask]>
To: [log in to unmask]
Sent: Fri, Oct 23, 2009 10:24 am
Subject: Re: [TN] [spam] RE: [TN] ENIG Issue

Hi Werner - there is a very good Dye & Pry testing procedure in the 

Appendices of the IPC 7093 specification on Bottom Terminated Components 

which includes the use of LN2. I have not observed the use of LN2 to 

confound the testing results.



Dave







Werner Engelmaier <[log in to unmask]> 

Sent by: TechNet <[log in to unmask]>

10/22/2009 05:46 AM

Please respond to

TechNet E-Mail Forum <[log in to unmask]>; Please respond to

Werner Engelmaier <[log in to unmask]>





To

[log in to unmask]

cc



Subject

Re: [TN] [spam] RE: [TN] ENIG Issue













 Hi Inge,

Yes, I have done 'Dye & Pry.'

The 'prying' part is not easy for large components. I did it starting at 

the corners working piecemeal around the 4 sides.

LN2 is a god idea?I do not see how it would cause misleading results, 

please explain.

Werner





 



 



-----Original Message-----

From: Hernefjord Ingemar <[log in to unmask]>

To: [log in to unmask]

Sent: Thu, Oct 22, 2009 4:44 am

Subject: [TN] [spam] RE: [TN] ENIG Issue





















By the way, speaking SJ issues, has anyone of you experience from Die & 

Pray 

technology, like the one described by some guys, who tested large game 

boards, 

see figur 9 and 10, dye and pry testing? It's not easy to pry so large 

BGAs. 

What kind of tools etc do you use? Myself, I had to dip the board under 

test in 

LN2 before prying off the superBGA. That's not good, the low temperature 

can 

mislead the result. 

/Inge



http://www.celestica.com/uploadedFiles/Home/PBfree_process_paper.pdf



 



-----Original Message-----

From: TechNet [mailto:[log in to unmask]] On Behalf Of Werner Engelmaier

Sent: onsdag 21 oktober 2009 15:51

To: [log in to unmask]

Subject: Re: [TN] ENIG Issue



 Hi Vladimir,

Maybe we should simply drop the name 'Black Pad' entirely-too much baggage 



and 

confusion.

Maybe we should refer to them by their failure modes and damage 

mechanisms-solderability issues due to 'galvanic corrosion', brittle 

fracture 

due to P-enrichment, brittle fracture due to 'any other cause applicable.

Werner



 



 



-----Original Message-----

From: [log in to unmask]

To: Werner Engelmaier <[log in to unmask]>; [log in to unmask]

Sent: Wed, Oct 21, 2009 7:39 am

Subject: Re: [TN] ENIG Issue



















   Werner,



Yes, I agree that there are two different phenomena BP and BF, but I can 

not 

agree on the statement that the root cause for BF(brittle fracture) is 

high P 

content. 



Regards,



Vladimir

SENTEC

11 Canadian Road, Unit 7.

Scarborough, ON M1R 5G1

Tel: (416) 899-1882

Fax: (905) 882-8812

www.sentec.ca





From:  Werner Engelmaier <[log in to unmask]>



Date: Tue, 20 Oct 2009 23:59:34 -0400

To: <[log in to unmask]>; <[log in to unmask]>

Subject: Re: [TN] ENIG Issue









 Vladimir,



Indeed you sent me that ATOTECH paper, but I have several references that 

disagree with their definition, as well as others that agree with the 

Atotech 

paper.



There seem to be (at least) 2 different 'defects' at work-one with 

hyper-galvanic corrosion of the Ni during Au-plating causing soldering 

problems, 

and another causing brittle separation due to a weakened interface cause 

by too 

much P.



Are we in agreement on this?



I do not really care what you call either of them-clearly the root cause 

is 

different in these cases and so is what needs to be done.



Clearly, what we need is for the IPC to form a committee to provide proper 





definitions and 'names.'



Werner











 











 







-----Original Message-----



From: [log in to unmask]



To: TechNet E-Mail Forum <[log in to unmask]>; Werner Engelmaier 

<[log in to unmask]>



Sent: Tue, Oct 20, 2009 11:23 pm



Subject: Re: [TN] ENIG Issue



























Werner,







We've been through it several times already. As far as I know, BP was 

defined as 





a case of poor Ni-P plating with cavitation present in the layer. I think 

I sent 





you an old ATOTECH paper on the topic a while ago.







Regards,







Vladimir







SENTEC



11 Canadian Road, Unit 7.



Scarborough, ON M1R 5G1



Tel: (416) 899-1882



Fax: (905) 882-8812



www.sentec.ca











-----Original Message-----



From: Werner Engelmaier <[log in to unmask]>



Date:         Tue, 20 Oct 2009 22:57:21 



To: <[log in to unmask]>



Subject: Re: [TN] ENIG Issue







 Hi Vladimir,







Then we are not communicating.







Please explain to me what YOU mean by 'BP failure'.







When I say 'BP failure', I mean it is because too much P between the Ni 

and the 



IMC layers has weakened the bond leading to brittle separation on 

sufficient 



loading. I do not differentiate as to the cause(s) for too much P. For me 

they 



describe a damage mechanism.







You can similar appearance with too much and too little P.







Werner























 























 















-----Original Message-----







From: [log in to unmask]







To: Werner Engelmaier <[log in to unmask]>; [log in to unmask]







Sent: Tue, Oct 20, 2009 10:44 pm







Subject: Re: [TN] ENIG Issue



















































   Werner,















You just confirmed what I said in my previous e-mail. You customer got 

failure 



with black appeared pads, but it wasn't BP failure. Similar appearance 

doesn't 



mean the same mechanism.















Regards,















Vladimir







SENTEC







11 Canadian Road, Unit 7.







Scarborough, ON M1R 5G1







Tel: (416) 899-1882







Fax: (905) 882-8812







www.sentec.ca































From:  Werner Engelmaier <[log in to unmask]>



















Date: Tue, 20 Oct 2009 22:16:40 -0400















To: <[log in to unmask]>; <[log in to unmask]>















Subject: Re: [TN] ENIG Issue











































 Hi Vladimir,











I have one client who experienced 'Black Pad' after 9(!) soldering 

operations. 



The P-content got progressively worse; it peaked with the EDS spikes for P 



being 





as high as those for Sn.











Werner



































 



































 























-----Original Message-----











From: [log in to unmask]











To: TechNet E-Mail Forum <[log in to unmask]>; Werner Engelmaier 



<[log in to unmask]>











Sent: Tue, Oct 20, 2009 10:07 pm











Subject: Re: [TN] ENIG Issue



































































Werner,































With all due respect, I don't think you are right.































Regards,































Vladimir















SENTEC















11 Canadian Road, Unit 7.















Scarborough, ON M1R 5G1















Tel: (416) 899-1882















Fax: (905) 882-8812















www.sentec.ca















































-----Original Message-----















From: Werner Engelmaier <[log in to unmask]>















Date:         Tue, 20 Oct 2009 22:01:35 















To: <[log in to unmask]>















Subject: Re: [TN] ENIG Issue































 Hi George,















\While what you say in the first paragraph is correct, the second 

paragraph is 















not.















'Black Pad' is not an all-or-nothing proposition. The seeds are sown at 

the 















Ni-plating (not the Au-plating) with the P-codeposition. However, multiple 



or 















lengthy expositions to high soldering temperatures result in more Ni being 



















dissolved to form IMCs leaving ever more P behind. This can create 'Black 

Pad' 















where none existed before.















Werner















































 















































 































-----Original Message-----















From: George Milad <[log in to unmask]>















To: [log in to unmask]















Sent: Tue, Oct 20, 2009 9:52 pm















Subject: Re: [TN] ENIG Issue















































































































































































As always as soon as there is a solderability issue with ENIG, "Black pad" 



 















comes up. This is a problem because it does not allow for further 















investigation.  Everyone accepts since this is ENIG then it must be black 

pad.















 















If this was a black pad issue the back side should have exhibited the same 



 















problem. BP occurs during the plating of the gold on top of the Ni. BP 















cannot  differentiate one side from the other.















 















Do not accept BP as the answer and keep investigating.















 















 















Regards















George Milad















George Milad















National Accounts  Manager for Technology















Uyemura International Corp (UIC)















249 Town Line Rd 















Southington CT 06489















[log in to unmask]















Cell: (516) 901  3874































---------------------------------------------------















Technet Mail List provided as a service by IPC using LISTSERV 15.0















To unsubscribe, send a message to [log in to unmask] with following text in















the BODY (NOT the subject field): SIGNOFF Technet















To temporarily halt or (re-start) delivery of Technet send e-mail to 















[log in to unmask]: SET Technet NOMAIL or (MAIL)















To receive ONE mailing per day of all the posts: send e-mail to 















[log in to unmask]: SET Technet Digest















Search the archives of previous posts at: http://listserv.ipc.org/archives















Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 



for 















additional information, or contact Keach Sasamori at [log in to unmask] or 















847-615-7100 ext.2815















-----------------------------------------------------































































 















































---------------------------------------------------















Technet Mail List provided as a service by IPC using LISTSERV 15.0















To unsubscribe, send a message to [log in to unmask] with following text in















the BODY (NOT the subject field): SIGNOFF Technet















To temporarily halt or (re-start) delivery of Technet send e-mail to 















[log in to unmask]: SET Technet NOMAIL or (MAIL)















To receive ONE mailing per day of all the posts: send e-mail to 















[log in to unmask]: SET Technet Digest















Search the archives of previous posts at: http://listserv.ipc.org/archives















Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 



for 















additional information, or contact Keach Sasamori at [log in to unmask] or 















847-615-7100 ext.2815















-----------------------------------------------------



















































 























 















---------------------------------------------------



Technet Mail List provided as a service by IPC using LISTSERV 15.0



To unsubscribe, send a message to [log in to unmask] with following text in



the BODY (NOT the subject field): SIGNOFF Technet



To temporarily halt or (re-start) delivery of Technet send e-mail to 



[log in to unmask]: SET Technet NOMAIL or (MAIL)



To receive ONE mailing per day of all the posts: send e-mail to 



[log in to unmask]: SET Technet Digest



Search the archives of previous posts at: http://listserv.ipc.org/archives



Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 



for 



additional information, or contact Keach Sasamori at [log in to unmask] or 



847-615-7100 ext.2815



-----------------------------------------------------















 









 





---------------------------------------------------

Technet Mail List provided as a service by IPC using LISTSERV 15.0

To unsubscribe, send a message to [log in to unmask] with following text in

the BODY (NOT the subject field): SIGNOFF Technet

To temporarily halt or (re-start) delivery of Technet send e-mail to 

[log in to unmask]: SET Technet NOMAIL or (MAIL)

To receive ONE mailing per day of all the posts: send e-mail to 

[log in to unmask]: SET Technet Digest

Search the archives of previous posts at: http://listserv.ipc.org/archives

Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 



for 

additional information, or contact Keach Sasamori at [log in to unmask] or 

847-615-7100 ext.2815

-----------------------------------------------------



---------------------------------------------------

Technet Mail List provided as a service by IPC using LISTSERV 15.0

To unsubscribe, send a message to [log in to unmask] with following text in

the BODY (NOT the subject field): SIGNOFF Technet

To temporarily halt or (re-start) delivery of Technet send e-mail to 

[log in to unmask]: SET Technet NOMAIL or (MAIL)

To receive ONE mailing per day of all the posts: send e-mail to 

[log in to unmask]: SET Technet Digest

Search the archives of previous posts at: http://listserv.ipc.org/archives

Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 



for 

additional information, or contact Keach Sasamori at [log in to unmask] or 

847-615-7100 ext.2815

-----------------------------------------------------







 





---------------------------------------------------

Technet Mail List provided as a service by IPC using LISTSERV 15.0

To unsubscribe, send a message to [log in to unmask] with following text in

the BODY (NOT the subject field): SIGNOFF Technet

To temporarily halt or (re-start) delivery of Technet send e-mail to 

[log in to unmask]: SET Technet NOMAIL or (MAIL)

To receive ONE mailing per day of all the posts: send e-mail to 

[log in to unmask]: SET Technet Digest

Search the archives of previous posts at: http://listserv.ipc.org/archives

Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 



for additional information, or contact Keach Sasamori at [log in to unmask] or 



847-615-7100 ext.2815

-----------------------------------------------------





---------------------------------------------------

Technet Mail List provided as a service by IPC using LISTSERV 15.0

To unsubscribe, send a message to [log in to unmask] with following text in

the BODY (NOT the subject field): SIGNOFF Technet

To temporarily halt or (re-start) delivery of Technet send e-mail to 

[log in to unmask]: SET Technet NOMAIL or (MAIL)

To receive ONE mailing per day of all the posts: send e-mail to 

[log in to unmask]: SET Technet Digest

Search the archives of previous posts at: http://listserv.ipc.org/archives

Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 

for 

additional information, or contact Keach Sasamori at [log in to unmask] or 

847-615-7100 ext.2815

-----------------------------------------------------



---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to 
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 
for additional information, or contact Keach Sasamori at [log in to unmask] or 
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential 
information, privileged material (including material protected by the 
solicitor-client or other applicable privileges), or constitute non-public 
information. Any use of this information by anyone other than the intended 
recipient is prohibited. If you have received this transmission in error, 
please immediately reply to the sender and delete this information from 
your system. Use, dissemination, distribution, or reproduction of this 
transmission by unintended recipients is not authorized and may be 
unlawful.


---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2