TECHNET Archives

September 2009

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
Linda Langley <[log in to unmask]>
Date:
Fri, 18 Sep 2009 09:07:39 -0500
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Subject:
From:
"David D. Hillman" <[log in to unmask]>
X-cc:
TechNet E-Mail Forum <[log in to unmask]>
In-Reply-To:
Content-Type:
text/plain; charset="US-ASCII"
MIME-Version:
1.0
Parts/Attachments:
text/plain (172 lines)
Hi Linda - what soldering processes have you been thru and/or trying to 
do?

Dave



"Linda Langley" <[log in to unmask]> 
09/18/2009 09:00 AM

To
"TechNet E-Mail Forum" <[log in to unmask]>, <[log in to unmask]>
cc

Subject
RE: [TN] Black Pad






We are having solderability issues, and the pads are black.

Linda Langley CIT
Training Specialist
Jabil Circuit
248-292-6176

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of David D. Hillman
Sent: Friday, September 18, 2009 9:54 AM
To: [log in to unmask]
Subject: Re: [TN] Black Pad

Hi Rudy - actually, if the copper and tin form an intermetallic phase 
during your first pass thru the reflow oven (which they should) then you

would have solderability issues during subsequent soldering operations.

Dave Hillman
Rockwell Collins
[log in to unmask]




R Sedlak <[log in to unmask]> 
Sent by: TechNet <[log in to unmask]>
09/18/2009 08:44 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
R Sedlak <[log in to unmask]>


To
[log in to unmask]
cc

Subject
Re: [TN] Black Pad






Linda:
Actually, it is quite possible to get black immersion Tin.   It comes
from 
running a bath with an excess of Cupric Copper in it.   I wrote a
article 
on how to monitor Cupric Copper in immersion Tin baths to avoid this in
a 
recent PCD&F magazine.

The black color should not affect solderability, as it is actually 
immersion Copper on top of the Tin.
Rudy Sedlak
RD Chemical Company

--- On Fri, 9/18/09, Linda Langley <[log in to unmask]> wrote:

From: Linda Langley <[log in to unmask]>
Subject: [TN] Black Pad
To: [log in to unmask]
Date: Friday, September 18, 2009, 3:12 AM

I know we have had this subject many times before so I did go to the
archives and still can't find an answer. My question, is Black Pad only
associated with ENIG? Is it possible with immersion Tin?

 

Linda Langley CIT

Training Specialist

Jabil Circuit

248-292-6176


---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to 
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 
for additional information, or contact Keach Sasamori at [log in to unmask]
or 
847-615-7100 ext.2815
-----------------------------------------------------



 

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to 
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 
for additional information, or contact Keach Sasamori at [log in to unmask]
or 
847-615-7100 ext.2815
-----------------------------------------------------


---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------


---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2