This very day, I couldn't stay aside but had to do something to help the
production guys. So, I took a fresh, naked and qualified board from another
source and did this:
Put one of our problem boards beside the reference board, both on bottom of
a larg well box, i.e. no fans blowing, nor any evacuation. Sprayed both
simultaneosly. Inspected them after one hour at room temp. The reference
board was absolutely perfect, while the other was matte! Had a look in a
microscope. The bad guy had thousands of microscopic inclusions and even
superficial voids, the reference was perfect. Noticed that the bad boards
have a much coarser (looks like the net pattern after screen printing)green
sheet (solder mask) and numerous voids already before spraying. What is your
opinion?
/Inge
----- Original Message -----
From: "Inge" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Sunday, August 23, 2009 9:53 PM
Subject: Re: [TN] Manual spraying
> Not likely, it's a fact that the weather is a bit unstable these days, but
> the barometric pressure, temperature and RH does not (fortunately) vary
> within minutes or even hours just now. The cans are weight checked and are
> all marked with same symbols on the bottom. I'm little disturbed by the
> abscense of the traditional steel ball, which use to be in most spray cans
> for painting or coating. Too much shaking, what do you mean?
>
> Inge
>
> ----- Original Message -----
> From: "Roger Stoops" <[log in to unmask]>
> To: "'TechNet E-Mail Forum'" <[log in to unmask]>; "'Inge'"
> <[log in to unmask]>
> Sent: Sunday, August 23, 2009 9:31 PM
> Subject: RE: [TN] Manual spraying
>
>
>> Sorry I'm late on this, and I haven't read all of the thread, but
>>
>> Sounds like the variation may be in the environment (temp, RH, barometric
>> pressure and such), or the can is almost empty/almost full/not shaken
>> enough/too much. Are these parameters being followed as well? Devil's
>> always lurking in those itty-itty details. If already checked, then
>> pardon
>> this ole' geezer...
>>
>> Roger
>>
>> (BTW, back to work doing board design again! Woo-hoo!)
>>
>> -----Original Message-----
>> From: TechNet [mailto:[log in to unmask]] On Behalf Of Inge
>> Sent: Sunday, August 23, 2009 3:07 PM
>> To: [log in to unmask]
>> Subject: Re: [TN] Manual spraying
>>
>> Yes, variations with same cans.
>> OK, will try baking.
>> Yes, from same fabricator.
>> Mystery.
>>
>> One of our old foxes, experienced process engineer, you've met him, made
>> a
>> try,
>> At first, the wet coating was crystal clear, but successively throughout
>> room drying, the
>> coating changed character, and became matte.
>>
>> Will let you know.
>>
>> Inge
>>
>>
>>
>> ----- Original Message -----
>> From: "Graham Naisbitt" <[log in to unmask]>
>> To: <[log in to unmask]>
>> Sent: Sunday, August 23, 2009 6:35 PM
>> Subject: Re: [TN] Manual spraying
>>
>>
>>> Inge
>>>
>>> All from the same can?
>>>
>>> If no, then I suspect some incomplete curing or "residual board
>>> contaminants" might be the problem.
>>>
>>> Try baking the problem boards for around 8 hours at 80C, leave them to
>>> revert to room temp and try again. If problem persists, then there you
>>> probably need to run FTIR to figure what is there causing the problem.
>>>
>>> Also, are they from the same board fabricator? If not, check ROSE to
>>> see
>>> if there is a difference.
>>>
>>> If yes, then have the batch checked - it is possible that there has
>>> been
>>> a labelling issue.
>>>
>>> Let me know
>>>
>>> Regards
>>>
>>> Graham Naisbitt
>>>
>>> Email: [log in to unmask]
>>> Phone: +44 (0)12 5252 1500
>>> Web: www.gen3systems.com
>>>
>>> On 21 Aug 2009, at 12:48, Hernefjord Ingemar wrote:
>>>
>>>> Nick,
>>>> we have done tests today, same operator, same boards, same cans, same
>>>> everything. Most boards get a clear, deep and nice look, but suddenly
>>>> we
>>
>>>> get a greyish coating, quite matte!
>>>>
>>>> Q1: what spray angle do you recommend?
>>>> Q2: what spray pattern do you recommend? Zig-zag, up-and-down, side-
>>>> to-side or what?
>>>> Q3: is the room RH of importance?
>>>> Q4: is the process sensitive to laminar flow and if so, what level is
>>>> critical?
>>>>
>>>> Inge
>>>>
>>>>
>>>>
>>>>
>>>> -----Original Message-----
>>>> From: TechNet [mailto:[log in to unmask]] On Behalf Of Nicholas
>>>> Redgrave-Plumb
>>>> Sent: fredag 21 augusti 2009 12:31
>>>> To: [log in to unmask]
>>>> Subject: Re: [TN] Manual spraying
>>>>
>>>> The only way I can see for the propellant causing this kind of problem
>>>> is if the nozzle of the spray can is too close to the substrate whilst
>>>> spraying. I note several suggestions in the posted responses of
>>>> expensive elevated IR curing ovens etc. for IB31 but these are really
>>>> not necessary as this material is dry to the touch/"tack" dry in only
>>>> minutes, dry in 24 hours and cured/fully optimised in 7 days. This
>>>> would
>>
>>>> undoubtedly be accelerated by an elevated cure but it shouldn't really
>>>> be necessary. So all you should really need is simple drying cabinet
>>>> at
>>>> ambient temperature just to take the solvent vapours away.
>>>>
>>>> Otherwise, it could be "champagning" or "solvent-popping" which are
>>>> terms to describe a condition where the surface of the coating
>>>> material
>>>> partially cures leaving solvent still trapped inside the wet- film.
>>>> The
>>>> solvent has to go somewhere so it finds it's way out through the
>>>> surface
>>
>>>> and in doing so makes multiple small holes.
>>>>
>>>> To avoid this problem should be a matter of going back to basics.
>>>> Review the coating procedure, make sure the operators are properly
>>>> trained (and not getting the spray nozzle too close to the substrate).
>>>> If the volumes justify the use of a purpose-built spray booth for
>>>> conformal coating with intrinsic safety features and laminar air- flow/
>>>> extraction then it might be worth going in that direction.
>>>>
>>>> But there should be a simple solution to this problem because the
>>>> usage
>>>> of HumiSeal 1B31 globally, in both liquid and aerosol cans is massive.
>>>>
>>>> Nick Plumb
>>>> Gen3 Systems Limited
>>>> Farnborough, United Kingdom
>>>>
>>>> _________________________________
>>>>
>>>>
>>>> On 20 Aug 2009, at 19:17, Inge wrote:
>>>>
>>>>> Good Evening,
>>>>> we use small cans filled with 1B1 conformal coating for handspraying
>>>>> boards. The guys are not satisfied with the result, because sometimes
>>>>> the result is matte. Microscope photos show thousands of microscopic
>>>>> bubbles in the coating. I suspect that it's included driving gas. Or
>>>>> wrong handling the spray can.Anyone out there with experience? How do
>>>>> you avoid this problem?
>>>>> /Inge
>>>>> ---------------------------------------------------
>>>>> Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
>>>>> unsubscribe, send a message to [log in to unmask] with following text
>>>>> in
>>>>> the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt
>>>>> or (re-start) delivery of Technet send e-mail to [log in to unmask]
>>>>> : SET Technet NOMAIL or (MAIL)
>>>>> To receive ONE mailing per day of all the posts: send e-mail to
>>>>> [log in to unmask]
>>>>> : SET Technet Digest
>>>>> Search the archives of previous posts at:
>>>>> http://listserv.ipc.org/archives Please visit IPC web site
>>>>> http://www.ipc.org/contentpage.asp?Pageid=4.3.16
>>>>> for additional information, or contact Keach Sasamori at
>>>>> [log in to unmask] or 847-615-7100 ext.2815
>>>>> -----------------------------------------------------
>>>>
>>>> ---------------------------------------------------
>>>> Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
>>>> unsubscribe, send a message to [log in to unmask] with following text in
>>>> the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt
>>>> or
>>
>>>> (re-start) delivery of Technet send e-mail to [log in to unmask] : SET
>>>> Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
>>>> posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
>>>> archives of previous posts at: http://listserv.ipc.org/archives Please
>>>> visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
>>>> additional information, or contact Keach Sasamori at [log in to unmask] or
>>>> 847-615-7100 ext.2815
>>>> -----------------------------------------------------
>>>>
>>>> ---------------------------------------------------
>>>> Technet Mail List provided as a service by IPC using LISTSERV 15.0
>>>> To unsubscribe, send a message to [log in to unmask] with following text
>>>> in
>>>> the BODY (NOT the subject field): SIGNOFF Technet
>>>> To temporarily halt or (re-start) delivery of Technet send e-mail to
>>>> [log in to unmask] : SET Technet NOMAIL or (MAIL)
>>>> To receive ONE mailing per day of all the posts: send e-mail to
>>>> [log in to unmask] : SET Technet Digest
>>>> Search the archives of previous posts at:
>>>> http://listserv.ipc.org/archives
>>>> Please visit IPC web site
>>>> http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
>>>> information, or contact Keach Sasamori at [log in to unmask] or
>>>> 847-615-7100
>>>> ext.2815
>>>> -----------------------------------------------------
>>>
>>> ---------------------------------------------------
>>> Technet Mail List provided as a service by IPC using LISTSERV 15.0
>>> To unsubscribe, send a message to [log in to unmask] with following text
>>> in
>>> the BODY (NOT the subject field): SIGNOFF Technet
>>> To temporarily halt or (re-start) delivery of Technet send e-mail to
>>> [log in to unmask]: SET Technet NOMAIL or (MAIL)
>>> To receive ONE mailing per day of all the posts: send e-mail to
>>> [log in to unmask]: SET Technet Digest
>>> Search the archives of previous posts at:
>>> http://listserv.ipc.org/archives
>>> Please visit IPC web site
>>> http://www.ipc.org/contentpage.asp?Pageid=4.3.16
>>
>>> for additional information, or contact Keach Sasamori at [log in to unmask]
>>> or
>>
>>> 847-615-7100 ext.2815
>>> -----------------------------------------------------
>>
>> ---------------------------------------------------
>> Technet Mail List provided as a service by IPC using LISTSERV 15.0
>> To unsubscribe, send a message to [log in to unmask] with following text in
>> the BODY (NOT the subject field): SIGNOFF Technet
>> To temporarily halt or (re-start) delivery of Technet send e-mail to
>> [log in to unmask]: SET Technet NOMAIL or (MAIL)
>> To receive ONE mailing per day of all the posts: send e-mail to
>> [log in to unmask]: SET Technet Digest
>> Search the archives of previous posts at:
>> http://listserv.ipc.org/archives
>> Please visit IPC web site
>> http://www.ipc.org/contentpage.asp?Pageid=4.3.16
>> for additional information, or contact Keach Sasamori at [log in to unmask]
>> or
>> 847-615-7100 ext.2815
>> -----------------------------------------------------
>>
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at [log in to unmask] or
> 847-615-7100 ext.2815
> -----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|