TECHNET Archives

August 2009

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
Date:
Mon, 3 Aug 2009 07:12:35 -0500
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, "Stadem, Richard D." <[log in to unmask]>
Subject:
From:
"Stadem, Richard D." <[log in to unmask]>
Content-Transfer-Encoding:
base64
In-Reply-To:
Content-Type:
text/plain; charset="utf-8"
MIME-Version:
1.0
Parts/Attachments:
text/plain (1 lines)
Ian, caps are mine.



3.9.3 Gold Removal- Gold shall be removed:

• From at least 95% of the surface to be soldered of the

through-hole component leads with

2.5 μm [0.0984 mil] or more of gold.

• From 95% of all surfaces of SURFACE MOUNT components to be soldered

regardless of gold thickness.

• From the surface of solder terminals plated with 2.5 μm

[0.0984 mil] or more of gold.

A double tinning process or dynamic solder wave may be

used for gold removal.



-----Original Message-----

From: TechNet [mailto:[log in to unmask]] On Behalf Of Fox, Ian

Sent: Monday, August 03, 2009 2:47 AM

To: [log in to unmask]

Subject: Re: [TN] AW: [TN] AW: [TN] FORMULA FOR DETERMINING GOLD PERCENTAGE IN A SOLDER JOINT



Last time I looked at J-std-001 (and IEC 61191 is a virtual carbon copy of it), gold removal is only required on through hole, to which I read wave soldered, components when the gold thickness is >2,5um. Personally if its an electrolytic gold finish I'll double dip tin to remove the gold regardless. Whilst the wave will scavenge the gold off the lead in the hole, assuming the pin/hole ratio isn't too tight, it will typically leave it in the top 10% of the hole and lead to premature crack formation



RegardsIan Fox

Lead Materials and Process Engineer

Aero Engine Controls

A Rolls-Royce plc and Goodrich Corporation Joint Venture





-----Original Message-----

From: TechNet [mailto:[log in to unmask]] On Behalf Of Joyce Koo

Sent: 31 July 2009 18:06

To: [log in to unmask]

Subject: Re: [TN] AW: [TN] AW: [TN] FORMULA FOR DETERMINING GOLD PERCENTAGE IN A SOLDER JOINT



Who ever made doc and approved it should get shot at... seriously.  Not a Friday joke. 



-----Original Message-----

From: TechNet [mailto:[log in to unmask]] On Behalf Of Jeremias, Michael

Sent: Friday, July 31, 2009 12:17 PM

To: [log in to unmask]

Subject: [TN] AW: [TN] AW: [TN] FORMULA FOR DETERMINING GOLD PERCENTAGE IN A SOLDER JOINT



Unfortunately it is not (!) a typo from me . The document  DIN EN  61191-1 contains  this  value  2,5 µm . But I am not confident, that this   is low enough for any process cases so we use  for PTH the same rule as above  as mentioned below

Sincerely 



Michael  Jeremias



-----Ursprüngliche Nachricht-----

Von: TechNet [mailto:[log in to unmask]] Im Auftrag von Joyce Koo

Gesendet: Donnerstag, 30. Juli 2009 12:22

An: [log in to unmask]

Betreff: Re: [TN] AW: [TN] FORMULA FOR DETERMINING GOLD PERCENTAGE IN A SOLDER JOINT



Must be a typo. Should be 0.25 micron? 10 micro-inches? 

--------------------------

Sent using BlackBerry





----- Original Message -----

From: TechNet <[log in to unmask]>

To: [log in to unmask] <[log in to unmask]>

Sent: Thu Jul 30 04:26:14 2009

Subject: [TN] AW: [TN] FORMULA FOR DETERMINING GOLD PERCENTAGE IN A SOLDER JOINT



IEC 61191-1

chapter  6.2.2 contains  the  rules

< 1,4% Volume Au, <  3% Wt Au in the final solder interconnection 

< 2,5 µm for  PTH Wave soldering  (I am not confident, that this   is low enough for any process cases so we use  for PTH the same rule as above)



You have to take into consideration solder paste volume(stencil-thickness), wetted Au-surface, wetted Au thickness



Own investigations  show, that Au brittelness may  occure from  1,6% Vol and really will occure from 2,3% Vol. 



 







Sincerly 



Michael Jeremias   

Industrial Engineering (OPPI41)

Electronics Production

((( Defence Electronics

EADS Deutschland GmbH

89077 Ulm

Tel.: +49 (0) 7 31.3 92-5533

Fax:     +49 (0) 7 31.3 92-73 15

E-Fax: +49 (0) 7 31.3 92-20 5533

P Before printing, think about the environment ! 



mailto: [log in to unmask]

EADS Deutschland GmbH

Registered Office: Ottobrunn

District Court of Munich HRB 107 648

Chairman of the Supervisory Board: Dr. Thomas Enders Managing Directors: Dr. Stefan Zoller (chairman), Michael Hecht This E-mail and any attachment(s) to it are for the addressee's use only.

It is strictly confidential and may contain legally privileged information. No confidentiality or privilege is waived or lost by any mistransmission.

If you are not the intended addressee, then please delete it from your system and notify the sender immediateley. You are hereby notified that any use, disclosure, copying or any action taken in reliance on it is strictly prohibited and may be unlawful. - Thank you.



---------------------------------------------------

Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815

-----------------------------------------------------



---------------------------------------------------------------------

This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful.



---------------------------------------------------

Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815

-----------------------------------------------------



---------------------------------------------------

Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815

-----------------------------------------------------



---------------------------------------------------------------------

This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful.



---------------------------------------------------

Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815

-----------------------------------------------------



--------------------------------------------------------------------------

This message (and any attachment) is confidential and is intended for the named recipient only.

If you receive it in error please e-mail back the sender and permanently delete the original message and any copies.

Rolls-Royce Goodrich Engine Control Systems Limited.

Registered Office: Moor Lane, PO Box 31, Derby, DE24 8BJ.

Registered in England No. 06686268.

--------------------------------------------------------------------------



---------------------------------------------------

Technet Mail List provided as a service by IPC using LISTSERV 15.0

To unsubscribe, send a message to [log in to unmask] with following text in

the BODY (NOT the subject field): SIGNOFF Technet

To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)

To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest

Search the archives of previous posts at: http://listserv.ipc.org/archives

Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815

-----------------------------------------------------


ATOM RSS1 RSS2