Kevin, if you can sacrifice a sample, preying off the component is a way to
get a very exact way to study voids. If the voids are adjacent to the solder
pad, which is often the case, the separation use to be just there. Very
large components, e.g. superBGAs, can not be removed this way, of course.
Inge
----- Original Message -----
From: "Glidden, Kevin" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Tuesday, August 25, 2009 8:29 PM
Subject: [TN] x-ray to estimate solder voiding
I am looking to have a couple of PCBs x-rayed to estimate the solder voiding
on the bottom only center pad of an SMT component. Can anyone recommend a
place?
Off line answers OK.
Thank you,
Kevin Glidden
Manufacturing Engineer
Luminescent Systems Inc.
Lebanon, NH 03766
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|