Just a thought, are you 100% certain that the features which you have
shown are not caused by scoring/scratching/handling on the surface of
the section? Could be some contact on the delicate sample surface
between final polish and observation, perhaps during etch or rinse
steps, or even during mounting onto a slide for viewing (dirt of the
sample press)? This could explain the continuation of a feature from the
solder joint into surrounding mould resin or soldermask.
Would be worth ruling out and again SEM inspection of the sample would
clarify. Would also be happy to take a quick look at them in the SEM for
you if you don't have access.
Kind regards,
Stewart
Stewart McCracken
MCS Ltd.
t. +44(0)131 440 9090
f. +44(0)131 440 9085
e. [log in to unmask]
w. www.themcsgroup.co.uk
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Gabriela
Sent: 04 July 2009 08:01
To: Administrator
Subject: [TN] Weird solder joints
Dear all,
By cross sectioning BGA solder joints on a failed assembly, I found that
the
suspected joints are not uniform and that they contain unusual
separation
areas.
I suspect mixed assembly and/or bad reflow profile.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------