I have seen this too many times before. It is simple solder bridging of adjacent pads with lead-free solder. Too much paste was printed, and too much pressure was used to place the components.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Karen Tellefsen
Sent: Friday, June 12, 2009 9:26 AM
To: [log in to unmask]
Subject: [TN] Strange tin "migration" under OFN soldered with no-clean SAC305 solder paste
One of our technical service engineers asked me about a strange migration
phenomenon one of our customers observed under passives and QFN's that have
been soldered with one of our no-clean SAC305 solder pastes. I've attached
an X-ray picture of a QFN exhibiting this strange failure, but I don't know
how it can be posted so you can look at it.. Further analysis after
removing the component showed that the shadows in the X-ray picture is
caused by a black material containing tin. The boards were conditioned 85°C
85%RH for 500 hr, but no voltage was applied. This phenomenon was not
observed under QFPs (not surprising), and seems to be independent of reflow
profile used. Additionally, the customer has not seen anything like this
with tin lead solder paste, however, the tin-lead solder pastes would have
a different fluxes. The tin "migration" is coming from both adjacent
solder joints, and there is no voltage applied, so it seems to be a
corrosion problem. Certainly QFN and big passives are good at trapping and
retaining water in the flux residue underneath them.
I've never seen anything like this; has anyone else out in TechNet land
seen this or have any ideas what caused this?
Thanks
Karen Tellefsen - Electrical Testing
[log in to unmask]
908-791-3069
(See attached file: Strange tin migration.JPG)
Enthone GmbH Geschäftsführer: Knut Balzer, Luc de Croo, Jürgen Dietrich Amtsgericht Düsseldorf HRB 45276
USt-Id-Nr. DE 811 205 946
This communication is for use by the intended recipient and contains information that may be privileged, confidential or copyrighted under applicable law. If you are not the intended recipient, you are hereby formally notified that any use, copying or distribution of this e-mail, in whole or in part, is strictly prohibited. Please notify the sender by return e-mail and delete this e-mail from your system. Unless explicitly and conspicuously designated as "E-Contract Intended", this e-mail does not constitute a contract offer, a contract amendment, or an acceptance of a contract offer. This e-mail does not constitute a consent to the use of sender's contact information for direct marketing purposes or for transfers of data to third parties.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|