TECHNET Archives

June 2009

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>
Date:
Mon, 15 Jun 2009 08:15:00 -0400
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Paul Reid <[log in to unmask]>
Subject:
From:
Paul Reid <[log in to unmask]>
Content-Transfer-Encoding:
quoted-printable
In-Reply-To:
Content-Type:
text/plain; charset="us-ascii"
MIME-Version:
1.0
Parts/Attachments:
text/plain (293 lines)
Hi Gaby,

My experience is that PWB reliability is a balance between copper
quality, material robustness and PWB design. In this case I would rule
out copper quality as a contributing factor to cratering. I would be
trying to balance material robustness and design attributes (including
PCB construction methods i.e. sequential lamination etc.) to reduce
cratering.

Thermal cycle testing of various materials and design attributes would
allow you to rank and select the best design/material combination for
your application. After that you would need to modify assembly methods
to reduce the risk of cratering.

I would make sure the surface finish application does not include a
thermal excursion. HASL and fused solder would add an additional thermal
excursion that, in some applications, have been quite detrimental.

Paul Reid



-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Werner Engelmaier /*
Sent: Saturday, June 13, 2009 11:34 PM
To: [log in to unmask]
Subject: Re: [TN] Corner ball pad cratering

 Hi Gaby,
That is exactly what I have been talking about.
Werner


 


 

-----Original Message-----
From: Gabriela <[log in to unmask]>
To: [log in to unmask]
Sent: Sat, Jun 13, 2009 5:01 pm
Subject: Re: [TN] Corner ball pad cratering










We had similar problems.
As you too, I saw it much more in ROHS applications.
And why not be frank-I will tell you what happened next:
Production did not  believe total loss, BGA's went through re-reflow-
for nothing ( oh, sorry, more cratered pads), removal (more cratered
pads), Lifted pads after removal, Pad repair on those we SAW, NEW BGA
soldering, failure again,due to pad/via open because the lifted pads
separated from the connectors (seen by X-ray).
Blabbering? Because I was and am FURIOUS!!!!!
SAC!!phui!
Gaby

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Vladimir Igoshev
Sent: Friday, June 12, 2009 9:51 PM
To: [log in to unmask]
Subject: Re: [TN] Corner ball pad cratering

I wouldn't be surprise if some of the joints are also partially cracked
right after re-flow. That is what I saw in the case I mentioned
yesterday.

In fact it was rather unusual to see partially craterred pads under
partially cracked balls.

As far as I know, my customer still tries to convince their CM to change
the re-flow profile (the cooling rate they used was way too high, but
they've never admitted that).

Regards,

Vladimir
SENTEC
SENTEC
11 Canadian Road, Unit 7.
Scarborough, ON M1R 5G1
Tel: (416) 899-1882
Fax: (905) 882-8812
www.sentec.ca


-----Original Message-----
From: Bev Christian <[log in to unmask]>

Date:         Fri, 12 Jun 2009 13:35:13 
To: <[log in to unmask]>
Subject: Re: [TN] Corner ball pad cratering


Chris,
We do extensive cross-sectioning to qualify any new reflow process and
all new Blackberry models. I have never, ever seen a pad cratering event
at this juncture - only after dropping during testing or from field
returns.
Bev

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Chris Mahanna
Sent: Friday, June 12, 2009 1:26 PM
To: [log in to unmask]
Subject: Re: [TN] Corner ball pad cratering

Genny and Bev,
Out of curiosity- are you sure that the cratering was not: induced
thermally (during reflow cool down), but did not manifest itself as a
problem until other mechanics came into play?
It just seems like that would be more common.
Chris

Chris Mahanna
Robisan Laboratory



-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Genny Gibbard
Sent: Friday, June 12, 2009 12:12 PM
To: [log in to unmask]
Subject: Re: [TN] Corner ball pad cratering

As always, Steve, you are a wealth of information.  That article is
perfect, thank you.  This seems to mirror what Amol said about doing a
1/4 of the length.  This article said to do an L shaped bead 2-6 balls
along each corner side.
Here are some photos to post.  Would you oblige?
BGA is 40mm per side.  PCB is ~1 ft sq.  A little bigger than what is
found in the typical blackberry, I think... Ball pitch is 1.27mm.
We believe the cause is mechanical, not thermal.
Thanks everyone.

Genny

-----Original Message-----
From: Steve Gregory [mailto:[log in to unmask]]
Sent: June 12, 2009 6:35 AM
To: TechNet E-Mail Forum; Genny Gibbard
Subject: RE: [TN] Corner ball pad cratering

Morning Genny,

Since you said you were going to look at corner bonding, here is a
really good article (if you haven't seen it already) that Michael
Kochanowski from Intel and Brian Toleno from Henkel did about it:

http://www.trafalgar2.com/documents/Technical_Articles/6.09-kochanowski.
pdf

Steve

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Genny Gibbard
Sent: Thursday, June 11, 2009 3:10 PM
To: [log in to unmask]
Subject: [TN] Corner ball pad cratering

Hello all,
If you have identified a BGA with corner ball pad cratering, what would
be your suggestions to correct this condition?
Our thoughts:
1.  We plan to evaluate our handling processes to reduce/remove
excessive flex/strain occurring around this part 2.  We plan to evaluate
corner bonding or underfilling for the BGA.

Which do you feel would be the best direction to go?  Do you have other
suggestions?
Thanks in advance for all your help

Genny

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------

---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential
information, privileged material (including material protected by the
solicitor-client or other applicable privileges), or constitute
non-public information. Any use of this information by anyone other than
the intended recipient is prohibited. If you have received this
transmission in error, please immediately reply to the sender and delete
this information from your system. Use, dissemination, distribution, or
reproduction of this transmission by unintended recipients is not
authorized and may be unlawful.

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask]
or 847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------



 


---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2