Hi Steve - as other members of Technet have detailed, the flux in a cored
wire is sealed in a metal container and is a very stable static
environment which results in flux cored wired having a shelf life of many,
many years. However, the flux cored wired manufacturers are required to
assign a shelf life by most specifications/quality systems and having a
short shelf life value results in increased consumable revenue stream. A
little bit of a technology and business protocol/ideology clash.
Individual companies do use longer shelf life allowances based on internal
testing data demonstrating that the flux cored wire meets the requirements
of the industry specifications.
Dave Hillman
Rockwell Collins
[log in to unmask]
Steve Gregory <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
06/05/2009 10:38 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
Steve Gregory <[log in to unmask]>
To
[log in to unmask]
cc
Subject
[TN] Flux cored wire solder shelf life
Well, we made it to Friday!
I'm going ask ya'll a couple of question that I think I know the answer
to, but I want to hear what you think.
Right now I'm in the midst of gathering up all my solder dross, expired
solder paste, and wire solder for a shipment to my recyclers. I noticed
we had a bunch of wire solder in the locker of our training room that
was really old, like it was manufactured back in February of 1997. The
alloy is 63/37, the flux core is a pretty active water soluble organic
acid.
The manufacturer says that shelf life for flux cored wire solder is
3-years. But when I took some of the solder and soldered with it, it
soldered absolutely fine. Wet and flowed out with no problems
whatsoever.
So my question is, have any of actually had any problems soldering with
flux cored wire solder because it was too old? Do you think that
manufacturers shelf life is realistic?
Steve
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|