TECHNET Archives

June 2009

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
Subject:
From:
Simon Huetter <[log in to unmask]>
Date:
Thu, 25 Jun 2009 10:43:46 +0200
In-Reply-To:
<6328A7F009D04BD0A68A09CF183A7169@ibmmrljzg6xbsk>
X-To:
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Simon Huetter <[log in to unmask]>
Parts/Attachments:
text/plain (189 lines)
             <[log in to unmask]>
                      
             <[log in to unmask]>
            
             <[log in to unmask]>
              <[log in to unmask]> 
 <6328A7F009D04BD0A68A09CF183A7169@ibmmrljzg6xbsk>
Content-Type: text/plain; charset="iso-8859-1"
Content-Transfer-Encoding: quoted-printable
MIME-Version: 1.0
X-OriginalArrivalTime: 25 Jun 2009 08:43:46.0642 (UTC) FILETIME=[0DAE8320:01C9F571]
X-NAI-Spam-Level: *
X-NAI-Spam-Score: 1
X-NAI-Spam-Report: 2 Rules triggered
	*  1 -- BAD_EMAIL_ADDRESS -- BODY: Contains a suspect email address
	*  0 -- RV3304 -- BODY: Version number


Hi Inge=2C

looking at the SEM pictures I would also say it's a pot issue.
The Copper load is to high=2C surface gets grainy and dull.

BTW=2C we have changed from SN100CL to SN100Ni+ and the Ni+
looks more shiny as CL.

Simon

> Date: Wed=2C 24 Jun 2009 20:27:52 +0200
> From: [log in to unmask]
> Subject: Re: [TN] SN100C I don't like the look of board pads
> To: [log in to unmask]
>=20
> Thanks=2C John and Mike=2C
> pot issue=2C sounds reasonable to me. I can't find a better guess=2C so I=
'll=20
> give them a hot pot shot.
> Thanks again=2C never been disappointed with TN=2C just couple of hours f=
rom=20
> question to answer.
> /Inge
>=20
>=20
> ----- Original Message -----=20
> From: "John Burke"=20
> To:=20
> Sent: Wednesday=2C June 24=2C 2009 4:59 PM
> Subject: Re: [TN] SN100C I don't like the look of board pads
>=20
>=20
>> Ugh=2C
>>
>> Last time I saw something like that was on a wave solder machine where t=
he
>> solder pump impeller was breaking up which lead to a very "rough" lookin=
g
>> joint with traces of iron.
>>
>> John Burke
>> (408) 515 4992
>>
>> -----Original Message-----
>> From: TechNet [mailto:[log in to unmask]] On Behalf Of Steve Gregory
>> Sent: Wednesday=2C June 24=2C 2009 6:41 AM
>> To: [log in to unmask]
>> Subject: Re: [TN] SN100C I don't like the look of board pads
>>
>> Morning Inge and Everybody!
>>
>> Got your pics posted Inge=2C and as usual=2C your pictures always give m=
e a
>> new window in which to see things. Here they are:
>>
>> http://stevezeva.homestead.com/files/SN100CSEM1.jpg
>>
>> http://stevezeva.homestead.com/files/SN100CSEM2.jpg
>>
>> I renamed your files and saved them as *.jpg files because my web page
>> doesn't allow me to use *.tif files. We've only used SN100 here a few
>> times=2C and you're right=2C ours looked just like regular 63/37 HASL. W=
e've
>> never had a SEM done on the boards we used=2C so I have nothing to compa=
re
>> your images to. But the boards we used were nice and shiny.
>>
>> Steve
>>
>> -----Original Message-----
>> From: TechNet [mailto:[log in to unmask]] On Behalf Of Hernefjord Ingemar
>> Sent: Wednesday=2C June 24=2C 2009 7:55 AM
>> To: [log in to unmask]
>> Subject: [TN] SN100C I don't like the look of board pads
>>
>> Hi all=2C
>>
>> will send pictures to Steve.
>> The two SEM images show SN100C boards that we got recently.
>> I don't like the look of the solder surface. Very grainy and with lots
>> of copper (darker spots). EDAX gives even fragments of iron. My first
>> thought was that the manufacturer had contaminated baths=2C which will b=
e
>> denied=2C of course. Anyway=2C my opinion is=2C that SN100C should be mo=
re
>> like ordinary tin/lead=2C i.e nearly zero copper and a more shiny
>> approach.
>>
>> /Inge
>> ---------------------------------------------------
>> Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
>> unsubscribe=2C send a message to [log in to unmask] with following text in
>> the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
>> (re-start) delivery of Technet send e-mail to [log in to unmask]: SET
>> Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
>> posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
>> archives of previous posts at: http://listserv.ipc.org/archives Please
>> visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=3D4.3.16 fo=
r
>> additional information=2C or contact Keach Sasamori at [log in to unmask] or
>> 847-615-7100 ext.2815
>> -----------------------------------------------------
>>
>> ---------------------------------------------------
>> Technet Mail List provided as a service by IPC using LISTSERV 15.0
>> To unsubscribe=2C send a message to [log in to unmask] with following text=
 in
>> the BODY (NOT the subject field): SIGNOFF Technet
>> To temporarily halt or (re-start) delivery of Technet send e-mail to
>> [log in to unmask]: SET Technet NOMAIL or (MAIL)
>> To receive ONE mailing per day of all the posts: send e-mail to
>> [log in to unmask]: SET Technet Digest
>> Search the archives of previous posts at: http://listserv.ipc.org/archiv=
es
>> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=3D4.=
3.16
>> for additional information=2C or contact Keach Sasamori at [log in to unmask]
g or
>> 847-615-7100 ext.2815
>> -----------------------------------------------------
>>
>> ---------------------------------------------------
>> Technet Mail List provided as a service by IPC using LISTSERV 15.0
>> To unsubscribe=2C send a message to [log in to unmask] with following text=
 in
>> the BODY (NOT the subject field): SIGNOFF Technet
>> To temporarily halt or (re-start) delivery of Technet send e-mail to=20
>> [log in to unmask]: SET Technet NOMAIL or (MAIL)
>> To receive ONE mailing per day of all the posts: send e-mail to=20
>> [log in to unmask]: SET Technet Digest
>> Search the archives of previous posts at: http://listserv.ipc.org/archiv=
es
>> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=3D4.=
3.16=20
>> for additional information=2C or contact Keach Sasamori at [log in to unmask]
g or=20
>> 847-615-7100 ext.2815
>> -----------------------------------------------------=20
>=20
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe=2C send a message to [log in to unmask] with following text =
in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to List=
[log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to Listserv@=
ipc.org: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archive=
s
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=3D4.3=
.16 for additional information=2C or contact Keach Sasamori at [log in to unmask]
rg or 847-615-7100 ext.2815
> -----------------------------------------------------

_________________________________________________________________
Hotmail: neu bis 70% schneller=2C bis 80% weniger Spam in der Inbox=2C viel=
 mehr Speicher & besserer Mobilzugriff!
http://www.microsoft.com/switzerland/windows/de/windowslive/products/hotmai=
l.aspx=

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2