TECHNET Archives

June 2009

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, Karen Tellefsen <[log in to unmask]>
Date:
Fri, 12 Jun 2009 12:31:49 -0400
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, "Wenger, George M." <[log in to unmask]>
Content-Transfer-Encoding:
quoted-printable
Subject:
From:
"Wenger, George M." <[log in to unmask]>
Content-Type:
text/plain; charset="iso-8859-1"
In-Reply-To:
MIME-Version:
1.0
Comments:
RFC822 error: <W> Invalid RFC822 field - "Karen,". Rest of header flushed.
Parts/Attachments:
text/plain (109 lines)
What is the surface finish on the QFN and what is t


Karen,



What is the surface finish on the QFN and what is the PCB surface finish?



Regards,

George

George M. Wenger

Andrew Solutions

Senior Principal FMA / Reliability Engineer

40 Technology Drive, Warren, NJ 07059

(908) 546-4531 [Office]  (732) 309-8964 [Cell]

[log in to unmask]

 



-----Original Message-----

From: TechNet [mailto:[log in to unmask]] On Behalf Of Karen Tellefsen

Sent: Friday, June 12, 2009 11:10 AM

To: [log in to unmask]

Subject: Re: [TN] Strange tin "migration" under OFN soldered with no-clean SAC305 solder paste



I though of creep corrosion also, but  flux contains no sulfur of halide.

That doesn't mean that there is no source of sulfur, but I don't know about

it.



Karen Tellefsen - Electrical Testing

[log in to unmask]

908-791-3069



fabrice pires <[log in to unmask]:



It make me think about creep corrosion phenomena. Is there any sulfur in

the residues?

Just an idea.





Karen Tellefsen a écrit :

> One of our technical service engineers asked me about a strange migration

> phenomenon one of our customers observed under passives and QFN's that

have

> been soldered with one of our no-clean SAC305 solder pastes. I've

attached

> an X-ray picture of a QFN exhibiting this strange failure, but I don't

know

> how it can be posted so you can look at it.. Further analysis after

> removing the component showed that the shadows in the X-ray picture is

> caused by a black material containing tin. The boards were conditioned

85°C

> 85%RH  for 500 hr, but no voltage was applied.  This phenomenon was not

> observed under QFPs (not surprising), and seems to be independent of

reflow

> profile used.  Additionally, the customer has not seen anything like this

> with tin lead solder paste, however, the tin-lead solder pastes would

have

> a different fluxes.   The tin "migration" is coming from both adjacent

> solder joints, and there is no voltage applied, so it seems to be a

> corrosion problem.  Certainly QFN and big passives are good at trapping

and

> retaining water in the flux residue underneath them.

>

> I've never seen anything like this; has anyone else out in TechNet land

> seen this or have any ideas what caused this?

>

> Thanks

>

> Karen Tellefsen - Electrical Testing

> [log in to unmask]

> 908-791-3069









Enthone GmbH  Geschäftsführer: Knut Balzer, Luc de Croo, Jürgen Dietrich  Amtsgericht Düsseldorf  HRB 45276

USt-Id-Nr. DE 811 205 946 





This communication is for use by the intended recipient and contains information that may be privileged, confidential or copyrighted under applicable law.  If you are not the intended recipient, you are hereby formally notified that any use, copying or distribution of this e-mail, in whole or in part, is strictly prohibited.  Please notify the sender by return e-mail and delete this e-mail from your system.  Unless explicitly and conspicuously designated as "E-Contract Intended", this e-mail does not constitute a contract offer, a contract amendment, or an acceptance of a contract offer.  This e-mail does not constitute a consent to the use of sender's contact information for direct marketing purposes or for transfers of data to third parties.



---------------------------------------------------

Technet Mail List provided as a service by IPC using LISTSERV 15.0

To unsubscribe, send a message to [log in to unmask] with following text in

the BODY (NOT the subject field): SIGNOFF Technet

To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)

To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest

Search the archives of previous posts at: http://listserv.ipc.org/archives

Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815

-----------------------------------------------------



------------------------------------------------------------------------------------------------

This message is for the designated recipient only and may

contain privileged, proprietary, or otherwise private information.  

If you have received it in error, please notify the sender

immediately and delete the original.  Any unauthorized use of

this email is prohibited.

------------------------------------------------------------------------------------------------

[mf2]



---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2