Hello John,
For me, photo 1 lets me think of paste slump combined with bad
coalescence of the paste during reflow, photo's 2 -4 only bad
coalescence as I know, induced by a too low temperature gradient in
the preheat section and/or too much moisture in the paste.
The first thing I would suggest is to perform the solder balling test
and if possible simultanuously the slump test. These tests rules out
the possibility of a bad paste lot.
Regards,
Peer Langeveld
Consultant Soft Soldering Processes
5502 VH 8 The Netherlands
2009/4/24 Mike Fenner <[log in to unmask]>:
> Looks like the most likely cause is lack of coalescence to me, possibly also
> too much paste.
> First though some housekeeping to get out of the way: Some water sol pastes
> are vulnerable to poor handling techniques, due to their susceptibility to
> humidity. All the rules on paste handling - do not leave lid off jar, do
> not keep recycling paste off/on the stencil, life on stencil, time after
> print to reflow etc - have to be observed. So those concerns are the first
> to be eliminated. Simplest thing to do is just try a fresh jar and 'walk'
> the boards down the line no delays.
>
> The next to check is profile. Water sol pastes usually respond best to
> straight ramp profiles, long soaks are undesirable. This is because the
> paste contains no natural "body" like a resin based no clean, they are all
> rheology agents and so are more likely to hot slump. The flux will also be
> more likely to exhaust itself with a long profile as there is no protective
> resin.
>
> As to why the problems seems amenable to pre-bake, this could be allied to
> the house-keeping issues out lined above, excess moisture, but seems
> disproportionate/unlikely. Or it could be a surface condition issue causing
> the flux components to bleed and carry solder particles with them. The
> baking would modify the surface energies and reduce bleeding. His would
> therefore be board issue.
> Likely there is no single magic bullet and combo solution will fix the
> problems
>
> Regards
>
> Mike Fenner
> Indium Corporation
>
>
> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]] On Behalf Of John Parsons
> Sent: Thursday, April 23, 2009 7:16 PM
> To: [log in to unmask]
> Subject: [TN] Solder Ball Problem
>
> I am trying to get to the root of a little solder ball problem. The problem
> is specific to a single part and was evident on the first run of this board
> a few months ago. We are seeing it again on this run although the common
> denominator here is that the PCB’s are all from the same production batch.
>
> It appears that the formation of solder balls can be reduced by pre-baking
> the PCB’s (100°C for 4-8 hrs) but not eliminated. The best results are
> obtained by pre-conditioning the PCB’s by running them through the reflow
> oven first, letting them cool, then print, populate and re-flow. The
> majority of balls now formed are dealt with at wash.
>
> The PCB’s are simple double sided, HASL finish. I suspect a problem with
> the solder finish (HASL) but what exactly that “problem” is I am not sure.
> FYI, paste is water soluble.
>
> http://stevezeva.homestead.com/files/Solder_ball_1.jpg - this photo is of a
> board that was pre-baked for about 4 hours @ 100°C, it was then printed and
> re-flowed. It does not matter if the 4 hour bake improved things you can
> see that the results are pretty spectacular.
>
> The following pictures are really more of the same except that these boards
> have been populated and washed.
>
> http://stevezeva.homestead.com/files/Solder_ball_2.jpg
>
> http://stevezeva.homestead.com/files/Solder_ball_3.jpg
>
> http://stevezeva.homestead.com/files/Solder_ball_4.jpg
>
> Any insight would be appreciated.
>
> (thanks to Steve for hosting the photos)
>
> Regards
> John Parsons
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at [log in to unmask] or
> 847-615-7100 ext.2815
> -----------------------------------------------------
>
>
> ***This email, its content, and any files transmitted with it, are intended solely for the addressee(s) and may be legally privileged and/or confidential. If you are not the intended recipient, please contact the sender by return and delete the material from any computer. Any review, retransmission, dissemination, or other use of, or taking of any action in reliance upon this information by persons or entities other than the intended recipient is prohibited.
>
> Messages sent via this medium may be subjected to delays, non-delivery, and unauthorized alteration. This email has been prepared using information believed by the author to be reliable and accurate, but Indium Corporation makes no warranty as to accuracy or completeness. Indium Corporation does not accept responsibility for changes made to this email after is was sent. Any opinions or recommendations expressed herein are solely those of the author. They may be subject to change without notice.***
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
> -----------------------------------------------------
>
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|