Hi Jim
Ouch!
sorry to say:
Forget for moment the word flux. Try thinking what your response would be if
someone said how reliable would a circuit be if we sprayed it with acid and
heated it to a couple of hundred degrees?
It is possible that your wash process will be good enough to 100% remove the
IA residues and/or reaction products from whatever it happened to touch
(liquid, spats fumes etc) from openly accessible surfaces, but unlikely.
It is highly improbable that it will remove the IA wicked into sleeve wires
and possibly elsewhere. If the sleeved wires are multi stranded - fine
diameter copper say - then they probably have a life measured in months.
Regards
Mike
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Jim West
Sent: Monday, March 09, 2009 11:45 PM
To: [log in to unmask]
Subject: [TN] Wrong flux used
During selective soldering, our operator used an IA flux (superior flux
75), which we normally use to dress up the soldering nozzle to create a
smooth flow of solder. The flux was applied by a spray fluxer. The
operator used the wrong bottle when reloading the spray fluxer.
We ran the boards through a wash system hoping to remove the IA flux.
The soldering operation involves discrete wires and I would think that the
flux would wick up under the wire insulation and not be reachable for
cleaning.
My questions are:
If the flux has wicked up under the wire insulator and can not be reached by
cleaning, will this type of flux
cause issues with the copper wire?
Will cleaning the boards be enough to say that no harm will be done, or
will this flux cause latent issues due to it's aggressiveness? (other
components were touched by this flux, i.e. SMT ceramic capacitors,
resistors)
Flux information
Superior soft soldering flux:
"The inorganic acid (IA) zinc chloride fluxes, commonly referred to as
"acid fluxes," are used for industrial soft soldering applications with
tin/lead, tin/silver, and other solder combinations. These fluxes typically
contain a combination of zinc chloride, hydrochloric acid, and ammonium
chloride and are used for soldering stainless steels, brass, copper, and
other metals."
Thanks,
Jim
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
***This email, its content, and any files transmitted with it, are intended solely for the addressee(s) and may be legally privileged and/or confidential. If you are not the intended recipient, please contact the sender by return and delete the material from any computer. Any review, retransmission, dissemination, or other use of, or taking of any action in reliance upon this information by persons or entities other than the intended recipient is prohibited.
Messages sent via this medium may be subjected to delays, non-delivery, and unauthorized alteration. This email has been prepared using information believed by the author to be reliable and accurate, but Indium Corporation makes no warranty as to accuracy or completeness. Indium Corporation does not accept responsibility for changes made to this email after is was sent. Any opinions or recommendations expressed herein are solely those of the author. They may be subject to change without notice.***
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|