TECHNET Archives

March 2009

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
Date:
Tue, 10 Mar 2009 11:21:29 -0500
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Karen Tellefsen <[log in to unmask]>
Content-type:
text/plain; charset=UTF-8
Subject:
From:
Karen Tellefsen <[log in to unmask]>
X-cc:
In-Reply-To:
Content-transfer-encoding:
base64
MIME-Version:
1.0
Parts/Attachments:
text/plain (1 lines)
The best is extraction and IC.  What do you have in your plant?



Karen Tellefsen - Electrical Testing

[log in to unmask]

908-791-3069







                                                                           

             "[log in to unmask]                                             

             m"                                                            

             <[log in to unmask]                                          To 

             M>                        [log in to unmask]                     

             Sent by: TechNet                                           cc 

             <[log in to unmask]>                                             

                                                                   Subject 

                                       Re: [TN] Wrong flux used            

             03/10/2009 11:11                                              

             AM                                                            

                                                                           

                                                                           

             Please respond to                                             

             [log in to unmask]                                             

                                                                           

                                                                           









What specific ionic cleanliness test should I have completed?  I'm told

there are several methods, with each giving different results.



Thanks for all the feedback up to this point!



Jim





Original Message:

-----------------

From: Karen Tellefsen [log in to unmask]

Date: Tue, 10 Mar 2009 07:43:29 -0500

To: [log in to unmask]

Subject: Re: [TN] Wrong flux used





Yuck!



The flux wicked up the wires, those wires will fail.  If the wires can be

replaced, you may be able to salvage the rest of the boards if you wash

them very thoroughly with hot DI water.  A prewash with saponifier wouldn't

hurt.  After washing,  you will need to ensure that all the flux was

removed by ionic cleaniless measurements or extraction and IC.



Good luck



Karen Tellefsen - Electrical Testing

[log in to unmask]











             Jim West

             <[log in to unmask]

             M>                                                         To

             Sent by: TechNet          [log in to unmask]

             <[log in to unmask]>                                          cc



                                                                   Subject

             03/09/2009 06:46          [TN] Wrong flux used

             PM





             Please respond to

              TechNet E-Mail

                   Forum

             <[log in to unmask]>

             ; Please respond

                    to

                 Jim West

             <[log in to unmask]

                    M>













During selective soldering, our operator used an IA flux (superior flux

75), which we normally use to dress up the soldering nozzle to create a

smooth flow of solder.  The flux was applied by a spray fluxer.  The

operator used the wrong bottle when reloading the spray fluxer.



We ran the boards through a wash system hoping to remove the IA flux.



The soldering operation involves discrete wires and I would think that the

flux would wick up under the wire insulation and not be reachable for

cleaning.



My questions are:



If the flux has wicked up under the wire insulator and can not be reached

by cleaning, will this type of flux

cause issues with the copper wire?



Will cleaning the boards be enough to say that no harm will be done, or

will this flux cause latent issues due to it's aggressiveness? (other

components were touched by this flux, i.e. SMT ceramic capacitors,

resistors)





Flux information

Superior soft soldering flux:

"The inorganic acid (IA) zinc chloride fluxes, commonly referred to as

"acid fluxes," are used for industrial soft soldering applications with

tin/lead, tin/silver, and other solder combinations. These fluxes typically

contain a combination of zinc chloride, hydrochloric acid, and ammonium

chloride and are used for soldering stainless steels, brass, copper, and

other metals."



Thanks,

Jim



---------------------------------------------------

Technet Mail List provided as a service by IPC using LISTSERV 15.0

To unsubscribe, send a message to [log in to unmask] with following text in

the BODY (NOT the subject field): SIGNOFF Technet

To temporarily halt or (re-start) delivery of Technet send e-mail to

[log in to unmask]: SET Technet NOMAIL or (MAIL)

To receive ONE mailing per day of all the posts: send e-mail to

[log in to unmask]: SET Technet Digest

Search the archives of previous posts at: http://listserv.ipc.org/archives

Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16

for additional information, or contact Keach Sasamori at [log in to unmask] or

847-615-7100 ext.2815

-----------------------------------------------------



---------------------------------------------------

Technet Mail List provided as a service by IPC using LISTSERV 15.0

To unsubscribe, send a message to [log in to unmask] with following text in

the BODY (NOT the subject field): SIGNOFF Technet

To temporarily halt or (re-start) delivery of Technet send e-mail to

[log in to unmask]: SET Technet NOMAIL or (MAIL)

To receive ONE mailing per day of all the posts: send e-mail to

[log in to unmask]: SET Technet Digest

Search the archives of previous posts at: http://listserv.ipc.org/archives

Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16

for additional information, or contact Keach Sasamori at [log in to unmask] or

847-615-7100 ext.2815

-----------------------------------------------------





--------------------------------------------------------------------

mail2web.com – What can On Demand Business Solutions do for you?

http://link.mail2web.com/Business/SharePoint



---------------------------------------------------

Technet Mail List provided as a service by IPC using LISTSERV 15.0

To unsubscribe, send a message to [log in to unmask] with following text in

the BODY (NOT the subject field): SIGNOFF Technet

To temporarily halt or (re-start) delivery of Technet send e-mail to

[log in to unmask]: SET Technet NOMAIL or (MAIL)

To receive ONE mailing per day of all the posts: send e-mail to

[log in to unmask]: SET Technet Digest

Search the archives of previous posts at: http://listserv.ipc.org/archives

Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16

for additional information, or contact Keach Sasamori at [log in to unmask] or

847-615-7100 ext.2815

-----------------------------------------------------


ATOM RSS1 RSS2