Hi Bill - I don't think Scott's dull solder joint appearance is due to
large lead dendrites formed by slow cooling as described by Mather and
Hagge. The Ag/Pd/PT termination finish can produce some "interesting"
microstructure phases which could be the root cause of the grainy, dull
solder joint appearance. Same basic principle but just another
microstructure phase root cause. Either way, your recommendation of Scott
chasing down the thermal history of the solder joints is spot on. I
actually have the original Mather/Hagge paper in our Technical Reference
library! That paper was published at the 6th Annual China Lake Soldering
Technology Seminar Proceedings in 1982. There is also an excellent
photograph of a large lead dendrite (due to slow cooling) causing solder
joint surface roughness in the International Tin Research Institutes
"Metallurgy of Soldered Joints in Electronics" Publication #708, page 36.
Dave
[log in to unmask]
Sent by: TechNet <[log in to unmask]>
01/14/2009 06:26 PM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
[log in to unmask]
To
[log in to unmask]
cc
Subject
Re: [TN] Dull and Grainy Leaded Solder Joints
What is the cooling rate of the grainy looking joints? Dull solder joints
was reported in the early days of vapor phase soldering, until Mather &
Hagge
of Rockwell Collins found that it was an artifact of slow cooling of the
joints which altered the grain structure of the solder joints.
Accelerating the
cooling rate solved the problem. Details can be found in their paper:
"Kinetics of Intermetallic Compound Formation and of Base Metal
Dissolution
into Molten Solder During Vapor Phase Soldering", John C. Mather and John
K.
Hagge, Collins Telecom Products Div'n., Cedar Rapids.
Perhaps Doug Pauls, Dave Hillman or Roy Keen would have a publication
citation where the paper can be found. I just have a photocopy of it.
Bill Kenyon
Global Centre Consulting
3336 Birmingham Drive
Fort Collins, CO 80526
Tel: 970.207.9586 Cell: 970.980.6373
**************A Good Credit Score is 700 or Above. See yours in just 2
easy
steps!
(
http://pr.atwola.com/promoclk/100000075x1215855013x1201028747/aol?redir=http://www.freecreditreport.com/pm/default.aspx?sc=668072%26hmpgID=62%26bcd=De
cemailfooterNO62)
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|