Hi Scott! Here are a couple of things to check - (a) your reflow profile,
specifically the temperature of the SMT inductors solder joints; (b) the
amount of solderpaste you are depositing for the SMT inductors. Ag/Pd/PT
terminations will produce a gritty/grainy solder joint appearance if the
finish is allowed to excessively "leach" into the solder joint. The
Ag/Pd/Pt termination is much happier to be in the solder than on the
component and you don't mention if you have a barrier layer on the
inductor to prevent leaching (I am guessing there is no barrier layer).
Also, if you have a lower solderpaste volume, you will increase the amount
of tin/silver and tin/palladium phases in the solder joint which could
lead to a rougher joint appearance. Good Luck.
Dave Hillman
Rockwell Collins
[log in to unmask]
"Newland, Scott" <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
01/13/2009 01:20 PM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
"Newland, Scott" <[log in to unmask]>
To
[log in to unmask]
cc
Subject
[TN] Dull and Grainy Leaded Solder Joints
We are suddenly seeing a rash of dull and grainy solder joints on SMT
inductors that use silver-palladium-platinum-glass frit terminations.
Otherwise the exterior of the joint looks good. The terminations as
supplied have no leaded or lead free solder or tin finish, just the
glass frit. In cross section the joint is also unique in that there is
no real IM layer and the grain structure near the joint is a bit odd.
The solder joints are fully re-flowed. All the other solder joints on
the CCA look good with no indication of solder process issues.
The vendor claims they have been supplying this type of termination for
years and nothing has changed, also this issue has just sprung up in the
last couple of months.
As far as we can tell the joints look different, but reliable.
Any suggestions or comments?
Scott Newland
Chief Mechanical Engineer - Fighter Enterprise
Harris GCSD
321 768 4272 (W)
321 720 1756 (C)
E-Mail [log in to unmask] <mailto:[log in to unmask]>
Do you have your CALCE log in? If not go to:
http://www.calce.umd.edu/accountrequest.html
<http://www.calce.umd.edu/accountrequest.html>
This information is only intended for the use of the individual or
entity named in this email. If you are not the intended recipient, you
are hereby notified that any disclosure, copying, distribution, or use
of the contents of this information is strictly prohibited. If you have
received this email in error, please notify me and delete it immediately
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|