DESIGNERCOUNCIL Archives

January 2009

DesignerCouncil@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
DesignerCouncil <[log in to unmask]>
X-To:
Designers Council Forum <[log in to unmask]>, Gary Koven <[log in to unmask]>
Date:
Thu, 22 Jan 2009 11:33:43 -0500
Reply-To:
"(Designers Council Forum)" <[log in to unmask]>, Andre Demers <[log in to unmask]>
Subject:
MIME-Version:
1.0
Content-Transfer-Encoding:
quoted-printable
Content-Type:
text/plain; charset="iso-8859-1"
From:
Andre Demers <[log in to unmask]>
Parts/Attachments:
text/plain (97 lines)
Hi Gary , 

We mark on our drawings a simple note : 
Total resistance of each line must not exceed xx ohms.

However , we usually design the board with this in mind and we 
know in advance what the limits are, so there are fewer surprises this way.

It's normal that the resistance is lower on the outer layers since the
plating adds another once of copper.

If your fabricator can't check DC trace resistance ,then I suggest you find one who can.

Best Regards,

Andre Demers C.I.D.
Senior PCB Designer 

cmrsummit Technologies 
310-733 boulevard St-Joseph 
Gatineau (Québec) J8Y 4B6 
Canada 

Telephone: 819.205.1185 
Toll Free: 877.428.1229 
Fax: 514.428.5953 

[log in to unmask] 
www.cmrsummit.com



-----Original Message-----
From: DesignerCouncil [mailto:[log in to unmask]] On Behalf Of Gary Koven
Sent: Thursday, January 22, 2009 10:25 AM
To: [log in to unmask]
Subject: [DC] Controlling DC trace resistance

We designed a board which has a number of critical connections where "power
delivery" and voltage drops can be deal breakers.  The board is FR-4
4101/21, 0.062in thick, 4 layer, 1oz Cu outer layers, 1oz Cu inner layers.
We were looking to control the DC trace resistance on the board by
controlling the copper thickness.

In order to verify that the copper thickness was correct on all layers, we
created 4 dogbone-type test coupons, one for each layer, 2.8in long and
terminating in two plated-through holes on each end.  We specified, on
drawing, a resistance of 70 milliohm nominal, 100 milliohm maximum, measured
between endpoints of the coupon using a 4-wire or Kelvin sense ohmmeter.  We
calculated the expected nominal resistance using the IPC-2221 tables and
curves.

During the build, we got a phone call from the fabricator about this
requirement, and we thought we had worked it out.  When the boards arrived,
we measured 40 milliohm on the outer layers and 100 milliohm on the inner
layers.  This wasn't what we expected.

When we called the fabricator to find out what measurements they got, we
didn't get a straight answer.  He started talking about dielectrics and
controlled impedance.  We gave up, because we're going to use the boards
anyway thanks to some lucky breaks in the way the software will work.

It was slightly disturbing to find that when we specified a critical
parameter on drawing, the fabricator didn't check this parameter or log the
results before delivering product.  DC resistance and controlled impedance
ain't the same animal.

Has anyone dealt with this requirement before and found a methodology to
better communicate it to a fabricator?


TIA and Best Regards,

===========================
Gary M. Koven, C.I.D.
Dynazign, Inc.
Charlotte, NC, USA
Veteran of the Marsh School

---------------------------------------------------------------------------------
DesignerCouncil Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF DesignerCouncil.
To temporarily stop/(restart) delivery of DesignerCouncil send: SET DesignerCouncil NOMAIL/(MAIL)
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
---------------------------------------------------------------------------------

---------------------------------------------------------------------------------
DesignerCouncil Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF DesignerCouncil.
To temporarily stop/(restart) delivery of DesignerCouncil send: SET DesignerCouncil NOMAIL/(MAIL)
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
---------------------------------------------------------------------------------

ATOM RSS1 RSS2