Dear :
依我們廠內作業經驗來看,1.金手指不能用酒精清潔.
2.含有Cl元素主
要原因是光手接觸金手指導致.
3.水清洗及回焊
爐過程中金手指有沒有被保護起來,
如果是水清
洗時與金手指接觸,那可以用高溫膠紙先貼起來.
Thank you for your support
Warmest Blessings
~~~~~~~~~~~~~~~~~~~~~~~~~~
Jimmy Kuo 郭 茂
Foxconn PCEG EPDI QE
TEL: 86-755-28128988 EXT: 86339
Mail:[log in to unmask]
~~~~~~~~~~~~~~~~~~~~~~~~~~
---------------------------------------------------------------------------------------------------------------------------------------------
本電子郵件及附件所載信息均為保密信息,受合同保護或依法不得洩漏。其內容僅供
指定收件人按限定範圍或特殊目的使用。 未經授權者收到此信息均無權閱讀、 使
用、 複製、洩漏或散佈。若您因為誤傳而收到本郵件或者非本郵件之指定收件人,請
即刻回覆郵件或致電NOTES郵件客服熱線 86-755-28101888分機 71120,並永久刪除此
郵件及其附件和銷毀所有複印件。謝謝您的合作!
This e-mail message together with any attachments thereto (if any) is
confidential, protected under an enforceable non-disclosure agreement,
intended only for the use of the named recipient(s) above and may contain
information that is privileged, belonging to professional work products or
exempt from disclosure under applicable laws.Any unauthorized review, use,
copying, disclosure, or distribution of any information contained in or
attached to this transmission is STRICTLY PROHIBITED and may be against the
laws. If you have received this message in error, or are not the named
recipient(s), please immediately notify the sender by e-mail or telephone
at Notes support hotline 86-755-28101888 EXT 71120 and delete this e-mail
message and any attached documentation from your computer. Receipt by
anyone other than the intended recipient(s) is not a waiver of any
attorney-client or work product privilege. Thank you!
---------------------------------------------------------------------------------------------------------------------------------------------
agale_2008
<[log in to unmask] TO:
OM> [log in to unmask]
CC:
主旨:
Re: [TGAsia] 金手指的污染问题
2008/12/12 PM
06:13
請回信 給 Asia
Committe Task
Group Forum
操作中的任何过程都会导致此类状况
在2008-12-11,HouToby <[log in to unmask]> 写道:
Hi All:
我们对金手指上的白色物质做了成分分析,发现其中含有Cl 元素,产品工艺流程:
回流焊---水清洗-----酒精清洁金手指-----装配, 现在还不知道怎么会有卤素跑到金
手指上的,各位大虾有什么高见
[IMAGE]
Best Regards!
Toby
Curtis Instruments China Co.,Ltd
86-512-68253070-859
86-512-68077767
The PCB consists between the Gold (Au) and the nickel (Ni) surface chlorine
(Cl). But there should be no chlorine (Cl)!. The Chlorine destruct the gold
surface and build an oxid. The oxid makes a high resistance.
使用新一代 Windows Live Messenger 轻松交流和共享! 立刻下载!