TECHNET Archives

December 2008

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
Date:
Tue, 9 Dec 2008 11:03:35 EST
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Subject:
From:
Joe Fjelstad <[log in to unmask]>
X-cc:
Content-Transfer-Encoding:
quoted-printable
Content-Type:
text/plain; charset="UTF-8"
MIME-Version:
1.0
Parts/Attachments:
text/plain (163 lines)
Thanks Rex
 
Kind regards, 
Joe
 
 
In a message dated 12/9/2008 4:06:06 A.M. Pacific Standard Time,  
[log in to unmask] writes:

JCAA/JG-PP Lead-Free Solder Project:
Vibration Test
Boeing  Electronics Materials and Processes Report - 582, Revision A
(EM/P-582,  Rev. A)
Contract No: BM3419-01
Prepared for ITB, Inc.
January 9,  2006

I have this paper and others. They are in the public domain. I  Googled the 
title of the paper and ended up at http://www.acqp2.nasa.gov/  where there are 
a multiplicity of papers on vibration results for differing  packages and 
differing alloys

Rex Waygood
Technical  Manager

PartnerTech Poole Ltd 
Benson Road
Poole
Dorset BH17  0RY
United Kingdom

Tel: +44 (0)1202 674333
Fax: +44 (0)1202  678028
DDI: +44 (0)1202 338222
Mob: +44 (0)7887  997403

[log in to unmask]
www.PartnerTech.co.uk

-----Original  Message-----
From: Leadfree [mailto:[log in to unmask]] On Behalf Of Deng,  Peter (Shenzhen)
Sent: 09 December 2008 09:16
To:  [log in to unmask]
Subject: Re: [LF] vibration testing of tin-lead and  lead-free solder joints

Joseph,

Your kind to dig out the link is  appreciated, I am interested in detail.
Thanks.

Regards / Peter  Deng
D +86(0)755 2671 0624
M ( +86) 138 2876 8267

-----Original  Message-----
From: Leadfree [mailto:[log in to unmask]] On Behalf Of Joe  Fjelstad
Sent: 2008年12月9日 4:45
To: [log in to unmask]
Subject: [LF]  vibration testing of tin-lead and lead-free solder  joints


Greetings  folks
Found this  on the wires  today... (Cut it earlier out but lost the link but 
I am  sure I am not  the only one who read it. However I can go dig it up if  
there is  interest)   
Why are we  still using lead-free solder again?  So it goes.... 
Joe
"Davide de  Maio of National Physical  Laboratory discussed the high 
frequency vibration  testing of tin-lead  and lead-free solder joints, with reference 
to automotive  and aerospace  electronics--a grim reminder that 80% of 
failures in airborne   electronics were attributable to vibration and shock. A test 
piece had  been  designed representing a single solder joint between two copper 
 components, which  was tested to failure at frequencies of 400Hz and  800Hz. 
A range of SAC  lead-free solders had been evaluated, with  tin-lead as a 
comparison. 
The  tin-lead solder outperformed the  lead-free examples, especially at the 
higher  frequency. In general,  failure occurred at or near the intermetallic 
interface,  which would be  expected to be the most stressed area. Of the SAC 
alloys,  performance at  400Hz was better the higher the silver content. 
Annealing of SAC  had a  deleterious effect on performance at both 400Hz and  
800Hz."
**************Make your life easier with all your friends, email,  and 
favorite sites in one place.  Try it now.  
(http://www.aol.com/?optin=new-dp&icid=aolcom40vanity&ncid=emlcntaolcom0000001
0)

------------------------------------------------------------------------------
-Leadfee  Mail List provided as a service by IPC using LISTSERV 1.8d To 
unsubscribe,  send a message to [log in to unmask] with following text in the BODY 
(NOT the  subject field): SIGNOFF Leadfree To temporarily stop/(start) delivery 
of  Leadree for vacation breaks send: SET Leadfree NOMAIL/(MAIL) Search 
previous  postings at: http://listserv.ipc.org/archives Please visit IPC web site  
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information,  
or contact Keach Sasamori at [log in to unmask] or 847-615-7100  ext.2815
------------------------------------------------------------------------------
-



Information  in this email and any attachments is confidential and intended 
solely for the  use of the individual(s) to whom it is addressed or otherwise 
directed. Please  note that any views or opinions presented in this email are 
solely those of  the author and do not necessarily represent those of the 
Company.
Finally,  the recipient should check this email and any attachments for the 
presence of  viruses. The Company accepts no liability for any damage caused by 
any virus  transmitted by this email.
All SGS services are rendered in accordance with  the applicable SGS 
conditions of service available on request and accessible  at  
http://www.sgs.com/terms_and_conditions.htm

------------------------------------------------------------------------------
-Leadfee  Mail List provided as a service by IPC using LISTSERV 1.8d To 
unsubscribe,  send a message to [log in to unmask] with following text in the BODY 
(NOT the  subject field): SIGNOFF Leadfree To temporarily stop/(start) delivery 
of  Leadree for vacation breaks send: SET Leadfree NOMAIL/(MAIL) Search 
previous  postings at: http://listserv.ipc.org/archives Please visit IPC web site  
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information,  
or contact Keach Sasamori at [log in to unmask] or 847-615-7100  ext.2815
------------------------------------------------------------------------------
-

------------------------------------------------------------------------------
-
The  information contained within this e-mail and any attachments contained 
therein  may be confidential and/or legally privileged and is for the use of 
the  intended recipient only. If you are not the intended recipient please 
delete  it from your system and notify the sender by return e-mail. The content of  
this e-mail may not be copied or disclosed to any third parties without prior 
 permission from the sender. 

E-mail is susceptible to data corruption,  interception, tampering and 
viruses. We do not accept any liability for any  such incidents or any consequences  
thereof.

------------------------------------------------------------------------------
-Leadfee  Mail List provided as a service by IPC using LISTSERV 1.8d
To unsubscribe,  send a message to [log in to unmask] with following text in
the BODY (NOT the  subject field): SIGNOFF Leadfree
To temporarily stop/(start) delivery of  Leadree for vacation breaks send: 
SET Leadfree NOMAIL/(MAIL)
Search  previous postings at: http://listserv.ipc.org/archives
Please visit IPC web  site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 
for additional  information, or contact Keach Sasamori at [log in to unmask] or 
847-615-7100  ext.2815
------------------------------------------------------------------------------
-


**************Make your life easier with all your friends, email, and 
favorite sites in one place.  Try it now. 
(http://www.aol.com/?optin=new-dp&icid=aolcom40vanity&ncid=emlcntaolcom00000010)

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2