Good description Mark
If I recall properly, having available excess of both metals on the two
sides is important as well for purple plague to occur. (e.g. Al wire on thick
gold pads or Au wire on thick Al pads) The problem was manifest in some early
Al wire bonding when relatively thick gold wire bond pads, common for gold
wire thermocompression and thermosonic bonding were used "as is" for Al wedge
bonding. Gold bonding on thin Al pads is very common these days.
Joe
In a message dated 11/5/2008 3:09:33 P.M. Pacific Standard Time,
[log in to unmask] writes:
Purple plague is an intermetallic alloy that is formed at the junction
of the Aluminum pad where the Gold bondwire is bonded. But this is not
a dendrite. It is a multi-crystalline growth that appears as a dark or
purple ring around the ball of the gold bondwire. Typically dendrites,
which will grow within a contaminated plastic IC, do not contain gold.
All it takes is the aluminum, moisture, and an electric field.
In the past purple plague has been generally caused by high temperature
whether or not the IC is powered. It usually causes an open circuit
(eventually) due to Kirkendahl voiding at the interface. With today's
very closely pitched bonding pads the purple plague growth may be able
to bridge between two adjacent bonding pads.
But again, this is not a dendrite. Dendrites need an electric field to
induce growth, purple plague occurs in the absence of an electric field.
It occurs at some rate continuously, but at normal operating
temperatures grows so slowly that it is not considered a primary factor
in calculating the lifetime of an IC.
mark
Mark Woolley
PTRL Laboratory
Avaya, 1300 West 120th Ave, Area 33, Westminster, CO, 80234
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Roberts, Jon
Sent: Tuesday, November 04, 2008 3:39 PM
To: [log in to unmask]
Subject: [TN] AL CU DENDRTIES INSIDE PLASTIC IC
Has anyone have knowledge or experience with AL Cu Dendrites growth in
plastic IC components? Reports or other information is appreciated,
Thanks, Jon
This communication is intended only for use by the addressee(s) named
herein and may contain business confidential and/or legally privileged
information. If you are not the intended recipient of this e-mail, you
are hereby notified that any dissemination, distribution, disclosure or
copying of this e-mail and its contents is strictly prohibited. If you
have received this e-mail in error, kindly notify the sender by replying
to this message. In addition, please permanently delete the message and
any attachments without copying or disclosing the contents. Thank you
for your cooperation.
THIS DOCUMENT AND/OR SHIPMENT MAY CONTAIN COMMODITY ITEMS, SOFTWARE OR
TECHNICAL DATA THAT IS CONTROLLED BY U.S. EXPORT LAW, AND MAY NOT BE
EXPORTED OUTSIDE THE UNITED STATES OR TO NON U.S. PERSONS WITHOUT THE
APPROPRIATE EXPORT LICENSE FROM EITHER THE U.S. DEPARTMENT OF STATE OR
DEPARTMENT OF COMMERCE.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
**************AOL Search: Your one stop for directions, recipes and all other
Holiday needs. Search Now.
(http://pr.atwola.com/promoclk/100000075x1212792382x1200798498/aol?redir=http://searchblog.aol.com/2008/11/04/happy-holidays-from
-aol-search/?ncid=emlcntussear00000001)
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|