TECHNET Archives

November 2008

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, Steve Gregory <[log in to unmask]>
Date:
Fri, 7 Nov 2008 14:58:39 -0500
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, "Wenger, George M." <[log in to unmask]>
Subject:
From:
"Wenger, George M." <[log in to unmask]>
Content-Transfer-Encoding:
quoted-printable
In-Reply-To:
Content-Type:
text/plain; charset="us-ascii"
MIME-Version:
1.0
Parts/Attachments:
text/plain (133 lines)
If you do run into Ron buy him too beers and I'll pay for
Steve,



If you do run into Ron buy him too beers and I'll pay for yours and his.

Great dendrite images.  I've seen silver dendrites grow off a silver

plated die paddle before but not off a die bond pad.



Regards,

George

George M. Wenger

Andrew Wireless Solutions

Senior Principal FMA / Reliability Engineer

40 Technology Drive, Warren, NJ 07059

(908) 546-4531 [Office]  (732) 309-8964 [Cell]

[log in to unmask]

 



-----Original Message-----

From: TechNet [mailto:[log in to unmask]] On Behalf Of Steve Gregory

Sent: Friday, November 07, 2008 2:51 PM

To: [log in to unmask]

Subject: [TN] DENDRITE GROWTH



Hi Jon!

 

Got your pictures posted. Go to:

 

http://stevezeva.homestead.com/files/Dendrites_1.jpg

 

http://stevezeva.homestead.com/files/Dendrites_2.jpg

 

http://stevezeva.homestead.com/files/Dendrites_3.jpg

 

Really nice photos of dendrites, beautiful fern-like structure.

 

Maybe one day we'll run into each and you can buy me that beer, but only

if I can buy you one too...

 

Steve



________________________________



From: Roberts, Jon [mailto:[log in to unmask]] 

Sent: Friday, November 07, 2008 12:58 PM

To: Steve Gregory

Subject: DENDRITE GROWTH







Steve, I was told you could post my pictures concerning the Dendrite

Growth inside of plastic ICs. I have enclosed the pictures two ways, in

the email body and on a .doc.  The information related to this I sent

out to the TechNet group this week. Thanks in advance I was told if I

see you to buy you a beer, Jon  



 



Enclosed is pictures  of the dendrites. 



 



Here is what the report stated associated with the pictures. 



 



EDX Spectra #1 is from the thick part of the dendrite on the bond pad

area, and shows a strong peak of silver (Ag) along with smaller peaks of

gold (Au), copper (Cu).   EDX Spectra #2 is the dendrite growth on the

Si surface; here the stronger peak is Ag with a trace of Cu.  The wire

ball is seen in EDX Spectra #3 and is primarily Au with smaller traces

of Ag.



 



This communication is intended only for use by the addressee(s) named

herein and may contain business confidential and/or legally privileged

information. If you are not the intended recipient of this e-mail, you

are hereby notified that any dissemination, distribution, disclosure or

copying of this e-mail and its contents is strictly prohibited. If you

have received this e-mail in error, kindly notify the sender by replying

to this message. In addition, please permanently delete the message and

any attachments without copying or disclosing the contents. Thank you

for your cooperation. 



THIS DOCUMENT AND/OR SHIPMENT MAY CONTAIN COMMODITY ITEMS, SOFTWARE OR

TECHNICAL DATA THAT IS CONTROLLED BY U.S. EXPORT LAW, AND MAY NOT BE

EXPORTED OUTSIDE THE UNITED STATES OR TO NON U.S. PERSONS WITHOUT THE

APPROPRIATE EXPORT LICENSE FROM EITHER THE U.S. DEPARTMENT OF STATE OR

DEPARTMENT OF COMMERCE. 





---------------------------------------------------

Technet Mail List provided as a service by IPC using LISTSERV 15.0

To unsubscribe, send a message to [log in to unmask] with following text

in

the BODY (NOT the subject field): SIGNOFF Technet

To temporarily halt or (re-start) delivery of Technet send e-mail to

[log in to unmask]: SET Technet NOMAIL or (MAIL)

To receive ONE mailing per day of all the posts: send e-mail to

[log in to unmask]: SET Technet Digest

Search the archives of previous posts at:

http://listserv.ipc.org/archives

Please visit IPC web site

http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional

information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100

ext.2815

-----------------------------------------------------





No virus found in this incoming message.

Checked by AVG - http://www.avg.com 

Version: 8.0.175 / Virus Database: 270.9.0/1773 - Release Date:

11/7/2008 9:08 AM

------------------------------------------------------------------------------------------------

This message is for the designated recipient only and may

contain privileged, proprietary, or otherwise private information.  

If you have received it in error, please notify the sender

immediately and delete the original.  Any unauthorized use of

this email is prohibited.

------------------------------------------------------------------------------------------------

[mf2]



---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2