TECHNET Archives

November 2008

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, "Woolley, Mark D. (Mark)" <[log in to unmask]>
Date:
Fri, 7 Nov 2008 10:06:17 -0600
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, "Roberts, Jon" <[log in to unmask]>
Subject:
From:
"Roberts, Jon" <[log in to unmask]>
Content-Transfer-Encoding:
quoted-printable
In-Reply-To:
Content-Type:
text/plain; charset="us-ascii"
MIME-Version:
1.0
Parts/Attachments:
text/plain (189 lines)
I appreciate all the responses and please continue. Anyone have the
knowledge where I can post the pictures for all of you to see?

I have enclosed an edited version to protect lab and component
manufacture. Let me know if you can read the document and see the
photos. 

Thanks again for all the inputs, Jon

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Woolley, Mark D.
(Mark)
Sent: Friday, November 07, 2008 9:39 AM
To: [log in to unmask]
Subject: Re: [TN] FW: [TN] AL CU DENDRTIES INSIDE PLASTIC IC

Corrosion of the aluminum conductors within the device which can lead to
dendrite formation as opposed to purple plague can be driven by moisture
that is captured within the device and phosphorous that is used in the
glass passivation over the IC to make it spread more easily.  Together,
they form phosphoric acid which corrodes aluminum quite well.  Other
contaminants need not be present, but will accelerate the corrosion
process if present.  This was a big issue with "canned" devices because
all moisture had to be excluded from the can prior to hermetically
sealing it.  The problem was reduced with the plastic encapsulation
because the plastic is molded around the IC and bondwires at
temperatures higher than the boiling point of water.  So most vapor is
excluded during the molding process.

Historically, the amount of phosphorous in the glass has not been well
controlled and an excess amount in the glass will damage the component
within.  Early ICs carried their own destruction mechanism!  Perhaps
control has gotten better in recent years.  I have been out of touch for
a while with this aspect of failures.
mark

Mark Woolley
PTRL Laboratory
Avaya,  1300 West 120th Ave,   Area 33,  Westminster, CO, 80234

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Syed Ahmad
Sent: Thursday, November 06, 2008 2:41 PM
To: [log in to unmask]
Subject: Re: [TN] FW: [TN] AL CU DENDRTIES INSIDE PLASTIC IC

Purple plague at the Au/Al interface would be aided by moisture and
contaminants like halides, Sb, etc., sometimes part of the molding
compound
as flame retardants.

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Whittaker, Dewey
(EHCOE)
Sent: Thursday, November 06, 2008 7:44 AM
To: [log in to unmask]
Subject: [TN] FW: [TN] AL CU DENDRTIES INSIDE PLASTIC IC

 

 


Subject: Re: [TN] AL CU DENDRTIES INSIDE PLASTIC IC

 

Purple plague is an intermetallic alloy that is formed at the junction

of the Aluminum pad where the Gold bondwire is bonded.  But this is not

a dendrite, it is a "Barny"cle.

Dewey

 

 

  It is a multi-crystalline growth that appears as a dark or

purple ring around the ball of the gold bondwire.  Typically dendrites,

which will grow within a contaminated plastic IC, do not contain gold.

All it takes is the aluminum, moisture, and an electric field.

 

In the past purple plague has been generally caused by high temperature

whether or not the IC is powered.  It usually causes an open circuit

(eventually) due to Kirkendahl voiding at the interface.  With today's

very closely pitched bonding pads the purple plague growth may be able

to bridge between two adjacent bonding pads. 

 

But again, this is not a dendrite.  Dendrites need an electric field to

induce growth, purple plague occurs in the absence of an electric field.

It occurs at some rate continuously, but at normal operating

temperatures grows so slowly that it is not considered a primary factor

in calculating the lifetime of an IC. 

 

mark

 

Mark Woolley

PTRL Laboratory

Avaya,  1300 West 120th Ave,   Area 33,  Westminster, CO, 8023


---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask]
or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------

This communication is intended only for use by the addressee(s) named herein and may contain business confidential and/or legally privileged information. If you are not the intended recipient of this e-mail, you are hereby notified that any dissemination, distribution, disclosure or copying of this e-mail and its contents is strictly prohibited. If you have received this e-mail in error, kindly notify the sender by replying to this message. In addition, please permanently delete the message and any attachments without copying or disclosing the contents. Thank you for your cooperation.                                                                                                        
THIS DOCUMENT AND/OR SHIPMENT MAY CONTAIN COMMODITY ITEMS, SOFTWARE OR TECHNICAL DATA THAT IS CONTROLLED BY U.S. EXPORT LAW, AND MAY NOT BE EXPORTED OUTSIDE THE UNITED STATES OR TO NON U.S. PERSONS WITHOUT THE APPROPRIATE EXPORT LICENSE FROM EITHER THE U.S. DEPARTMENT OF STATE OR DEPARTMENT OF COMMERCE.

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2