As usual Werner has made a very good observation, one that I was not going to get into but...
A failing PTH with a nickel surface finish will may have cracks that start from the nickel and propagates into toward the dielectric. This is a common failure where the nickel causes the initiation of the crack.
There in no evidence of nickel in the PTH. Therefore I think these cracks are wider at the inner edge because the barrel is bowing inward toward the center of the hole due to plastic deformation. There is X, Y and Z axis expansion during thermal excursions and I expect that the atypical cracks is due to an inward displacement or bowing of the PTH.
Other contributing factors to consider would be aggressive microetch of the XS, indium based solder, or microsectioning artifacts. I ruled out chemical attach, copper dissolution or inclusions based on the shape of the crack.
Best regards,
Paul
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Werner Engelmaier /*
Sent: Monday, October 06, 2008 4:26 PM
To: [log in to unmask]
Subject: Re: [TN] Barrel and Corner cracks in copper elctroplating
Hi Ido,
Quite frankly, what your pics show I have never seen before--this sure is the weirdest ever. Barrel cracks typically start on the resin-side of the barrel because of the way the barrel is loaded. This almost looks like some form of chemical attack.
Werner
-----Original Message-----
From: Ido Mashall <[log in to unmask]>
To: [log in to unmask]
Sent: Sat, 4 Oct 2008 4:41 am
Subject: Re: [TN] Barrel and Corner cracks in copper elctroplating
Sorry for the picture problems
I set it up now and its OK
http://www.drivehq.com/file/df.aspx/shareID4765976/fileID233954134/eo-d3497-
1.jpg
http://www.drivehq.com/file/df.aspx/shareID4765976/fileID233954135/es-c9633-
1.jpg
http://www.drivehq.com/file/df.aspx/shareID4765976/fileID233954138/as-d3715.
Jpg
Thanks for the inputs and for any more
Ido Mashall
http://www.beyond-materials.com/index-en.htm
Fax: +972-4-6376666, Tel: +972-77-2127172,
Mobile +972-52-5901114, www.beyond-materials.com
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Paul Reid
Sent: Saturday, October 04, 2008 12:52 AM
To: [log in to unmask]
Subject: Re: [TN] Barrel and Corner cracks in copper elctroplating
Hi Ido,
I cannot view the http site to which you have linked.
I get the following message:
"Free users cannot publish folders, files or web pages. Folders published by free users are for preview only; they will expire in 20 minutes.
It is a DriveHQ standard policy to only allow "trusted" users to publish.
This is to prevent "bad" users from pu
blishing inappropriate contents. Free
users are not considered trusted. A free user can upgrade to True User or Premium (Paid) User. To become a True user, you must register your account with a private domain company email address, or deposit at least $3 into your DriveHQ account."
I guess your 20 minutes are up and the picture are removed.
Usually we ask Steve Gregory to post TechNet pics on his site stevezeva.homestead.com. Can you send the pictures to Steve
([log in to unmask]) and ask him to post the pictures on his site so we can all view them?
Lead/free 260°C assembly produces a different type of barrel and corner crack than tin/lead 230°C. A 288°C float may be showing these somewhat unique failure modes.
Change in crack morphology may be a results of Cu bath contamination, brightener and chemistry maintenance, electrical properties (RMS ripple, racking, bussing, pulse etc) but material may also play a role in lead/free applications. Grid size is another variable that is expressing different failure modes in lead/free applications.
If I can view the 288°C induced corner and barrel cracks I will gladly comment on them.
Sincerely,
Paul Reid
Program Coordinator
PWB Interconnect Solutions Inc.
235 Stafford Rd., West, Unit 103
Nepean, Ontario
Canada, K2H 9C1
613 596 4244 ext. 229
Skype paul_reid_pwb
[log in to unmask] <mailto:[log in to unmask]>
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Ido Mashall
Sent: Friday, October 03, 2008 2:13 PM=0
ATo: [log in to unmask]
Subject: [TN] Barrel and Corner cracks in copper elctroplating
Hello technet
We are suffering a serious problem of barrel and corner cracks in the pattern copper plate bath.
Please look at the following pic. (all after 288C solder thermal stress)
http://www.drivehq.com/file/df.aspx/shareID4765976/fileID233954134/eo-d3497-
1.jpg
http://www.drivehq.com/file/df.aspx/shareID4765976/fileID233954135/es-c9633-
1.jpg
http://www.drivehq.com/file/df.aspx/shareID4765976/fileID233954138/as-d3715.
jpg
This very strange phenomenon occurs only in the second copper, and does not occur in the panel plated copper.
After testing all bath components, they seem to be ok. CVS is oK, hull cell is OK. It seems the copper lost its mechanical properties.
We are looking for possible contamination and changed the bath for a new fresh bath, and it happens again after a few days..
Does somebody have some idea why this cracks can occur? What other reasons..?
Thanks.
Ido Mashall
Fax: +972-4-6376666, Tel: +972-77-2127172,
Mobile +972-52-5901114, http://www.beyond-materials.com/index-en.htm
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
No virus found in this incoming message.
Checked by AVG - http://www.avg.com
Version: 8.0.173 / Virus Database: 270.7.5/1706 - Release Date: 03/10/2008
18:17
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail t o
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|