Hi Anand,
ENIG is Electroless Nickel Immersion Gold Plating & is not suitable for
Gold Wire Bonding as the thickness of Gold is only 3-8microinches & for
gold wire bonding you would need at least 30-40microinches. Soft Gold
Plating is an electroplating process which can be plated to the required
thickness without any issue, of course at a cost. However if you want to
use ENIG, then some of the Chemistry vendors provide what is called a
Nickel-Palladium-Gold where the bonding is to the Palladium & the gold
is very thin like the ENIG process. But this is suitable for Aluminium
Wire bonding,. Hope this helps. If you need more info pls feel free to
contact me......
Thanks & Best Regards,
Krishnan C
Director Of Quality
Sanmina-SCI Corporation (M) Sdn. Bhd.
Sama Jaya Free Industrial Zone
93450 Kuching, Sarawak, Malaysia.
Tel: 60 82 363 000 Ext 1602
Mobile: (6) - 012-8888-379
Fax: 60 82 363 527
E-mail: [log in to unmask]
"It is easier to do a job right than to explain why you didn't."
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Anand Paliwal
Sent: Thursday, September 25, 2008 3:07 AM
To: [log in to unmask]
Subject: [TN] Plating types
Hi all,
i am quite new to this community so pls help me.
What is the Difference between ENIG and Soft gold wire Bondable Plating
?
is the ENIG type of plating for soft wire bondable ?
i have COB on board so i want to specify Soft Gold wire bondable
plating but
my fab house gives ENIG.
Pls reply
Thanks
Anand
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
CONFIDENTIALITY
This e-mail message and any attachments thereto, is intended only for use by the addressee(s) named herein and may contain legally privileged and/or confidential information. If you are not the intended recipient of this e-mail message, you are hereby notified that any dissemination, distribution or copying of this e-mail message, and any attachments thereto, is strictly prohibited. If you have received this e-mail message in error, please immediately notify the sender and permanently delete the original and any copies of this email and any prints thereof.
ABSENT AN EXPRESS STATEMENT TO THE CONTRARY HEREINABOVE, THIS E-MAIL IS NOT INTENDED AS A SUBSTITUTE FOR A WRITING. Notwithstanding the Uniform Electronic Transactions Act or the applicability of any other law of similar substance and effect, absent an express statement to the contrary hereinabove, this e-mail message its contents, and any attachments hereto are not intended to represent an offer or acceptance to enter into a contract and are not otherwise intended to bind the sender, Sanmina-SCI Corporation (or any of its subsidiaries), or any other person or entity.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|