¡¡¡¡ÄãºÃ£¡Engelmaier,
¡¡¡¡Our supplier had provided their reliability report according to IPC
9701£¬the report shows the test duration is to 63.7% of the cumulative
failure distribution or 6000 thermal cycles. But at present I am more
concerned about the infant failure from external overload, like board warp
or mechanical shock.
¡¡¡¡Another question is why the weakest point is between nickel layer and
IMC layer. Could you give me some explanation about the failure mechanism of
the brittle fracture.
¡¡¡¡Best regards!
¡¡¡¡Min Jun
¡¡¡¡H3C process engineer
¡¡¡¡Tel:+86-010-82774234
¡¡¡¡
¡¡¡¡
****************************************************************************
***********
¡¡¡¡This e-mail and its attachments contain confidential information from
H3C, which is intended only for the person or entity whose address is listed
above. Any use of the information contained herein in any way (including,
but not limited to, total or partial
¡¡¡¡disclosure, reproduction, or dissemination) by persons other than the
intended recipient(s) is prohibited. If you receive this e-mail in error,
please notify the sender by phone or email immediately and delete it!
¡¡¡¡
****************************************************************************
************
¡¡¡¡
¡¡¡¡-----ÓʼþÔ¼þ-----
·¢¼þÈË: TechNet [mailto:[log in to unmask]] ´ú±í Werner Engelmaier /*
·¢ËÍʱ¼ä: 2008Äê9ÔÂ19ÈÕ 10:25
ÊÕ¼þÈË: [log in to unmask]
Ö÷Ìâ: Re: [TN] Copper balls/pins
¡¡¡¡
¡¡¡¡Nee hao Min Jun,
¡¡¡¡No, I am not surprised that you are having failures with copper pin
solder
¡¡¡¡joints--these pins are not compliant leads. What you essentially have is
a
¡¡¡¡leadless solder connection.
¡¡¡¡I sure wish these component suppliers would do their reliability
homework.
¡¡¡¡The 2 pdf's you make reference to either make nonsensical reliability
¡¡¡¡statements, or obliquely refer to IPC-9701 without giving ay results.
¡¡¡¡
¡¡¡¡Regards,
¡¡¡¡Werner Engelmaier
¡¡¡¡¿É¿¿ÐÔÏÈÉú
¡¡¡¡Engelmaier Associates, L.C.
¡¡¡¡Electronic Packaging, Interconnection and Reliability Consulting
¡¡¡¡7 Jasmine Run
¡¡¡¡Ormond Beach, FL 32174 USA
¡¡¡¡Phone: 386-437-8747, Cell: 386-316-5904
¡¡¡¡E-mail: [log in to unmask], Website: www.engelmaier.com
¡¡¡¡
¡¡¡¡
¡¡¡¡**************
¡¡¡¡Looking
¡¡¡¡for simple solutions to your real-life financial challenges? Check out
¡¡¡¡WalletPop for the latest news and information, tips and calculators.
¡¡¡¡
¡¡¡¡(http://www.walletpop.com/?NCID=emlcntuswall00000001)
¡¡¡¡
¡¡¡¡---------------------------------------------------
¡¡¡¡Technet Mail List provided as a service by IPC using LISTSERV 15.0
¡¡¡¡To unsubscribe, send a message to [log in to unmask] with following text
in
¡¡¡¡the BODY (NOT the subject field): SIGNOFF Technet
¡¡¡¡To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
¡¡¡¡To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
¡¡¡¡Search the archives of previous posts at:
http://listserv.ipc.org/archives
¡¡¡¡Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.
16 for additional information, or contact Keach Sasamori at [log in to unmask]
or 847-615-7100 ext.2815
¡¡¡¡-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|