TECHNET Archives

September 2008

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
Date:
Fri, 12 Sep 2008 06:34:28 -0700
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, "Whittaker, Dewey (EHCOE)" <[log in to unmask]>
Subject:
From:
"Whittaker, Dewey (EHCOE)" <[log in to unmask]>
Content-Transfer-Encoding:
quoted-printable
In-Reply-To:
Content-Type:
text/plain; charset="US-ASCII"
MIME-Version:
1.0
Parts/Attachments:
text/plain (206 lines)
That's why his designs are good to the last drop.
Dewey

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Mike Fenner
Sent: Friday, September 12, 2008 5:38 AM
To: [log in to unmask]
Subject: Re: [TN] exploding cercaps NTC

Inge: 
[Could be John is descended from the coffee branch of the family]

 :)

Regards 

Mike

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Hernefjord Ingemar
Sent: Friday, September 12, 2008 11:47 AM
To: [log in to unmask]
Subject: Re: [TN] exploding cercaps

Thanks for the input, John.
Your knowhow in this matter is unquestionable. I really appreciate that
you
gave our problem a minute.
(In fact, not our problem, I do consulting for another big company).
Inge
PS. It's Friday, and I feel for a little 'Maxwell' test: John, what is
the
basic equation for the magnetic flux in a electromagnetic coil? As
son-son-son of famous Maxwell, you must keep the magnetic
tradition....he-he

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of John Maxwell
Sent: den 12 september 2008 01:44
To: [log in to unmask]
Subject: Re: [TN] exploding cercaps

Inge,
I have included some comments added to your speculations based on my
experience and represent my observations only.

John

>Hi all,
>I have solved numbers of cercap issues, some easy tasks, others very 
>qualified. Now, in order to find the right track asap, I thought ; why 
>not utilize TN expertise? Alzo, my question:
>
>What is the failure mode most likely to be?
>
>FR4 backplanes, 4 mm thick, lots of pressfit connectors. Transient 
>protection by means of ceramic capacitors, size approx 8x6x1mm (LxWxT).
>SMT 60Sn. The catastrophic failures ALWAYS start at the end of the cap,

>from small microfumaroles to half ceramic body vaporized. From tiny 
>spots of soot on the FR4 to something that reminds of what happens when

>you are careless with your gas torch welder!  The board is warped, 
>about 2 mm along 200 mm. The board is torqued down flat with several 
>bolts. May not seem to result in a lot of tension, but ceramic 
>capacitors are very sensitive to axial/bend forces. I have cut out 
>samples about 25x100 mm, populated with 4-8 caps, then polished them 
>until only half thickness remains, then bent the samples slightly 
>('simulate' torque down). Out of a hundred, some caps developed a 
>obvious crack CLOSE to the end metallisation (Ag;Ni). The cracks are 
>always in parallel with the end metallisation and across whole width of

>cap body. EDS on the solder joints gives that the solder surface is 
>irregular and grainy, and contains small amounts of both Silver and 
>Nickel. The end metallisation is unusually thick with a 60-80 um Silver

>layer. On outside of this is some 2-5 um Nickel. The meniscus is 
>normal, which means very 'fat' in my opinion (most of us don't realise 
>yet, the benefit with meagre fillets). The failure occurs 
>stochastically in field use. Forgot to mention that the BaTiO is beige 
>and it's a 100k MLC. One and the same manufacturer.
>
>My speculations are:
>
>A. Mechanical force from curved/straightened board is root cause

(John Maxwell) Mechanical/flexure stresses are the most common root
cause of
MLCC failure but these are failures on a 4mm thick board.
This related to what Werner stated in is response, large fillets lead to
failure similar to mechanical/flexure cracks.

>B  Anomalous metallisation give local current issues which create 
>hotspots and finally sparks etc

(John Maxwell) At best a third order effect

>C. Solder metallurgy faulty, or fatigued, giving too high serial 
>resistance which gives local hotspots etc

(John Maxwell) See item B above

>D. Shorts or delaminations not likely, as the failues are always at the
end.

(John Maxwell) I agree

>E. Bad Silver adhesion not very common

(John Maxwell) Cap loss is the failure mode and not burning caps.

>F. Nickel with bad pretinning = high resistivity or loss of galvanic 
>contact not very likely either.

(John Maxwell) See item B above


>I know some of you have had many working days without sleep, because of

>puffing cercaps.

(John Maxwell) When I was a consultant I viewed puffing caps as my house
payment, retirement and tuition for my kids to go to school. As a user I
did
loose sleep.


>Thanks in advance
>
>Inge

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in
the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet
NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send
e-mail to [log in to unmask]: SET Technet Digest Search the archives of
previous posts at: http://listserv.ipc.org/archives Please visit IPC web
site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in
the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet
NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send
e-mail to [log in to unmask]: SET Technet Digest Search the archives of
previous posts at: http://listserv.ipc.org/archives Please visit IPC web
site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------


***This email, its content, and any files transmitted with it, are
intended solely for the addressee(s) and may be legally privileged
and/or confidential. If you are not the intended recipient, please
contact the sender by return and delete the material from any computer.
Any review, retransmission, dissemination, or other use of, or taking of
any action in reliance upon this information by persons or entities
other than the intended recipient is prohibited.

Messages sent via this medium may be subjected to delays, non-delivery,
and unauthorized alteration. This email has been prepared using
information believed by the author to be reliable and accurate, but
Indium Corporation makes no warranty as to accuracy or completeness.
Indium Corporation does not accept responsibility for changes made to
this email after is was sent. Any opinions or recommendations expressed
herein are solely those of the author. They may be subject to change
without notice.***

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2