Steve,
Actually, Ingemar is referring to a flying machine, although I saw one of those bikes the other day. Had to do a double-take.
I fly what is called a Powered Parachute [PPC], being suspended beneath 500 sq ft of nylon. Air speed is 30 mph. Altitude is nap of the earth to 10,000 ft, although much over 3-4,000 ft I feel 'naked'.
One sees the earth from a totally different perspective. Kind of like taking a 'color tour' in your recliner [if you are from an area that experiences the changes of color].
Steve
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Steve Gregory
Sent: Wednesday, August 20, 2008 8:10 AM
To: [log in to unmask]
Subject: Re: [TN] Wire bonding gurus ohoy!
Steve, you ride a Trike?
Last month when I was in Colorado for my IPC-7711/7721 certification, I got to go up in the Rocky Mountains National Park one day for a little sight-seeing. I came around a bend in the road and saw one of the coolest trikes I've ever seen! I just had to stop and learn more about it. The gentleman that owned it was really a nice guy and even let me sit on it:
http://stevezeva.homestead.com/files/Sitting_on_a_Spyder.jpg
Couldn't talk him into letting me take it on a spin though...darn it! ;^)
Steve
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Inge
Sent: Tuesday, August 19, 2008 12:45 PM
To: [log in to unmask]
Subject: Re: [TN] Wire bonding gurus ohoy!
Trikeman,
Y-O-U A-R-E A...A...A...hmmm....A D-O-U-N-U-T-!!!
That was the best I could find to praise you. Excellent. I buy every line.
Feel intuitively that your magic rod is working as always. Yup, have Al wedge, will try it. As you say, one lift is one too much. The customer of this laser optic device is worried. I don't know what they use it for, but reliability is no1, they pay for that.
'Cat-eye'...good word for the phenomenon. Just now we rather call it 'Cat-shit'. Tomorrow, I'll sit down with the customer and go through what you recommend. I will start with showing a photo taken from the sky from your trike and ask him to contribute with a little bag of sheckels for your petrol consumtion..he-he.
Now, besides joking, I bow and say thanks a lot. Hope I can do something for you too in du time.
Inge
----- Original Message -----
From: "Creswick, Steven" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Tuesday, August 19, 2008 9:57 AM
Subject: Re: [TN] Wire bonding gurus ohoy!
Ingemar,
I know that you have gone home for the evening, but this will be there in
the morning for you to ponder on.
It's my humble opinion that the 'cats-eye' pattern which you see is related
to the dominance of U/S energy in the North-South direction of the
transducer. It may sound counter-intuitive, but I believe you will find the
'cats-eye' runs East-West [perpendicular to the dominant mode of oscillation
of the capillary] - at least that is the way it is on my machines.
I have seen this before in GaAs, InGaN, etc - but usually it is also tied in
with cratering! Usually putting too much energy into the crystal ... or in
the case of Si, just putting too much energy into the bond.
With the exception of a small metallization lift in the upper right tip if
the 'iris', your metallization appears to be intact. It appears that the
bond seriously attempted to adhere.
A couple things that I have experienced with chrome-gold metallizations -
- actually a chrome-gold alloy, being very hard and almost impossible to
thermosonic gold bond to. i.e. - you are screwed !! Big time! Consider a
switch to aluminum wedge bonding, if you can
- gold layer not exhibiting good adhesion to the chrome layer, and comes off
during bonding leaving a nice little hole down to the chrome layer. Be
loving. Be gentle. Should bond like a dream if you can get enough bonded
area to meet pull strengths. Increase bonding temp?? Again, can you wedge
bond?
Neither of the above would seem to apply to your part, however.
I typically run with a 90° inner chamfer and an 8° face angle. The face
angle predominantly being dictated by the requirements of the second bond
surface - the softer the surface, the greater is my face angle. Not feeling
that the face angle comes into first bond parameters much other than by
bond-foot length.
I believe the 120° IC would provide a greater downward vector of
force/energy, but have not been running with that due to fear of ball
capture issues during bonding. Read as the 90° works fine, so am not going
to rock the boat.
I extensively use an SPT - Small Precision Tools UTS-51KJ-CM-1/16-16mm
15MTA - an 8° face angle, 90°IC, with 50µm hole. Am bonding 37.5µm wire on
100µm square pads 'til the cows come home'. When dealing with a lot of
LEDs, used a similar capillary with the same wire but on 75µm square pads.
Ran like a champ! Not an easy challenge to put down wire that large on
those smallish pads without cratering/lifting/etc.
I'm sure you have tried all the 'normal' stuff like:
- plasma cleaning to freshen up the surface.
- Compared old vs new lots.
- Contemplated running across the EDS to check for a preponderance of chrome
on the surface - although 2500A of Au may not do a good job of blocking out
the rest of the chrome from the signal electrons either.
- Verify heat column temps and clamping.
- verify they are not actually over-bonding [visual observation of bonds]
Ingemar, I am at a loss to think of anything else to jot down at the moment.
Hoping that sharing bonding tool info helps to some degree. You've not
really said if this is a new lot of die, or there was some other upstream
process change, etc. that you are investigating ....so I am still shooting
in the dark somewhat. You are probably like me in that 'many' bond lifts is
something like 1-2 out of a hundred or more :-) One is TOO many!
Steve
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Steve Gregory
Sent: Monday, August 18, 2008 8:30 AM
To: [log in to unmask]
Subject: Re: [TN] Wire bonding gurus ohoy!
Mornin' Inge!
Got your picture posted, but that's all the help I can offer...I know
nothing about wire bonding.
Your picture is here:
http://stevezeva.homestead.com/files/Wirebond.jpg
Steve
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Hernefjord Ingemar
Sent: Monday, August 18, 2008 4:13 AM
To: [log in to unmask]
Subject: [TN] Wire bonding gurus ohoy!
Hi all,
will send a picture to Steve for getting help.
Thermosonic 25um gold balls don't stick to the thinfilm gold on a optic
chip.
2,500A Au over 400A Cr. Bad yield, many balls lift. No contaminations
found.
Despite I have the good fishbone, I can't find out why the odd pattern
under lifted bals.
A guess is that the capillary have to steep chamfer angle, so that the
U/S mechanical energy becomes concentrated in the middle. Anyone with
similar experience?
Inge
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
THE INFORMATION CONTAINED IN THIS E-MAIL MESSAGE AND ANY ATTACHMENTS SENT
FROM GENTEX CORPORATION IS GENTEX CONFIDENTIAL INFORMATION INTENDED ONLY FOR
THE PERSONAL USE OF THE INDIVIDUAL OR ENTITY NAMED ABOVE. If you are not the
intended recipient, you are hereby notified that any review, distribution,
or copying of this communication is strictly prohibited. If you have
received this communication in error, please immediately notify the sender
by return e-mail, and delete this e-mail message and any attachments from
your computer. [gntx v.1]
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|