Thanks for the mention, Inge, but the figure I think you are referring to
(in http://www.ami.ac.uk/courses/topics/0268_wb/index.html) is labelled
"Thermosonic wire bond cause and effect diagram", and was developed for gold
bonding, rather than aluminium wedge. Not that the two would be vastly
different.
On the site, the fish-bone is attributed as "Eisenberg 1990". Unfortunately,
I can't immediately locate more of a reference - the page originated in
1997, and its sources are somewhere in my attic!
Regards, Martin
Martin Tarr
Martin Tarr Associates Ltd
+44 (0)1383 723989 phone
+44 (0)7831 550192 mobile
www.mtarr.co.uk
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Hernefjord Ingemar
Sent: Friday, August 15, 2008 9:12 AM
To: [log in to unmask]
Subject: Re: [TN] NiAu Specification for Al Wedge Wire Bonding
I forgot to tell who made the bone. Say thank you to Martin Tarr at AMI.
-----Original Message-----
From: Hernefjord Ingemar
Sent: den 15 augusti 2008 10:05
To: 'TechNet E-Mail Forum'
Subject: RE: [TN] NiAu Specification for Al Wedge Wire Bonding
Arnoud et netters,
I've finally found the troubleshooting fishbone for wirebonding. I will ask
Dr Gregory about presenting it on the Zevawall. Don't feel miserable when
you see it...wire bonding use to work without any of the fishbone problems.
Keep the bone, care not to loose it, worthful for production people.
Inge
-----Original Message-----
From: Hernefjord Ingemar
Sent: den 13 augusti 2008 13:12
To: 'TechNet E-Mail Forum'
Subject: RE: [TN] NiAu Specification for Al Wedge Wire Bonding
This is not a fishbone, but you can make a bone of it, if you fish...wish
Wire bonding trouble shooting list:
1. Wrong loop height
2. Improper wire diameter
3. Wire elongation not adapted to object.
4. Wire alloy (doping)
5. Wire age (some wires have limited shelf life) 6. Bonding tool radius 7.
Bonding tool face polish type 8. Bonding tool, build-up of debris in chamfer
and on face 9. Tool vibration amplitude and/or frequency inadequate 10.Bond
force not adequate 11.Bond time not adequate, frequency swing not correct
12.Microscopic damage on wire caused by burrs in the tool 13.Intermetallic
growth between wire and pad metallisation
(about 10 compounds known, some of which very brittle) 14.Impurities on
or in the bond pads, either they are thickfilm or PWB 15.Inadequate
metallisation thickness vs. dielectric thickness 16.The ultrasonic energy
causes delamination of bond pad metallisation 17.The wire vibrates too much
in the tool, wire gets microcracks and heel damage 18.The deformation of the
wedge/ball is not sufficient, or is overdone.
19.Insufficient number of microwelds
20.Outgassing of polymers or other stuff, which can cause bond lift or bad
bond yield 21.The bond pad micro structure (asperity)is too rough
22.Diffusion of metals or other stuff, which can change the characteristic.
23.Kirkendall voids, which makes bonds brittle and weak.
24.Maximum current exceeded in bond wire, can cause electro migration
25.Thermal moves that causes bond weakening through defects in the
crystalografic structure 26.Hydrogen bubbles in the metallisation.
27.Presence of halogens in the ambient atmosphere can reduce bond yield
28.Cratering in semiconductor bond pads, too far gone and the wire bond will
lift.
29.Fluorocarbons, chlorides or other residues from the semiconductor process
will disturb the bond process 30.The ultrasonic energy is not correctly
'grounded'(insufficient clamping)
Especially important for large boards 31.Some wires or PWBs or substrates
should be stored in dry nitrogen
until the day of wire bonding.
32.So called 'lubricants' may inhibit bond success, e.g. finger prints
33.Contaminations, from the machinery in automatic lines, can contaminate.
34.The superficial surface of Thickfilm gold or silver/palladium pads
contain too much of Si, Bi, or Cd 35.Corroded metallisation of bond pads.
36.Oxides on bond pads
37.Microscopic amounts of water (temporarily), from inadequate storage
38.Microscopic amounts of water from humid ambient
The list is from one of my technical reports, there may be something
missing...
Inge
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Hernefjord Ingemar
Sent: den 11 augusti 2008 14:05
To: [log in to unmask]
Subject: Re: [TN] NiAu Specification for Al Wedge Wire Bonding
Arnaud et TNetters,
I've not found the wirebonding fishbone, it's so tiny that my cats may have
eaten it all. How ever however, another fishbone may serve some of you, I'll
send it to Dr Gregory , and well packaged so that the custom people don't
feel the smell.
Ineg
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of arnaud grivon
Sent: den 15 mars 2007 14:51
To: [log in to unmask]
Subject: Re: [TN] NiAu Specification for Al Wedge Wire Bonding
Thanks for the cake, but coming back to the initial question, is there any
standardisation or good practices for the NiAu plating used for Al wedge
bonding?
Best regards,
A. Grivon
Hernefjord Ingemar a écrit :
> Arnoud,
>
> There is a lot to say, I send a good cake to start with ( 4Meg offline).
> If any further questions, send smoke signal. Trikeman is guru.
> Inge
>
> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]] On Behalf Of arnaud grivon
> Sent: den 14 mars 2007 16:01
> To: [log in to unmask]
> Subject: [TN] NiAu Specification for Al Wedge Wire Bonding
>
> Hello TechNet,
>
> A question for wire bonding gurus (and I know there are some).
> What are the NiAu specifications adapted for Al wedge wire bonding?
> Ni & Au thicknesses, electrolytic or electroless, roughness,
> hardness....
> Are there some normalized documents covering these aspects (IPC,
> MIL...)?
> Thanks in advance.
>
> Best regards,
>
> A. Grivon
>
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet
NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send
e-mail to [log in to unmask]: SET Technet Digest Search the archives of
previous posts at: http://listserv.ipc.org/archives Please visit IPC web
site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|