> Hallo Klaus,
> You focus on 5 possible causes for the Xbox 360 failures:
> (1) the higher thermal stress during Pb-free soldering (possibly at Tpeak
around 240 C)
A: that certainly is a concern, specifically because for larger BGAs, a peak
T of 240 is inadequate for reflow soldering of SAC solders;—however, if this
were the root cause, failures would happen before shipping or shortly
thereafter, and the failed SJs would be in the center of the BGA.;
> (2) the higher thermal stress during specified operation had been the main
> ones of several failure promoters.
> A: thermal stress is a poor descriptor—a high thermal expansion mismatch
> between BGA and PCB is the most likely cause—the thermal expansion mismatch is
> the product of component size, delta-CTE and delta-T; failures would be of SJs
> near the die or BGA periphery.
>
> (3) flaws in thermal board design (maybe no thermal steady state and
> transient simulations)
> A: see delta-T above.
> (4) flaws in material selection (of the type of Pb-free solder used)
> A: not much difference in the common Pb-free solder—however, the EU's Pb-ban
under RoHS is clearly a major contributor to the problem.
> (5) flaws of processing (maybe omission of an underfill under the BGA
> and/or non-optimal reflow solder profile
> A: see (1) above—the right underfill would help.
Regards,
Werner Engelmaier
Engelmaier Associates, L.C.
Electronic Packaging, Interconnection and Reliability Consulting
7 Jasmine Run
Ormond Beach, FL 32174 USA
Phone: 386-437-8747, Cell: 386-316-5904
E-mail: [log in to unmask], Website: www.engelmaier.com
**************
Looking for a car that's sporty, fun and fits in your budget?
Read reviews on AOL Autos.
(http://autos.aol.com/cars-BMW-128-2008/expert-review?ncid=aolaut00050000000017 )
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|