Amol,
The MSL is 3 - 168 hours. They are coming out of dry-packed, vacuum sealed
bags with date codes of 0749, 0801, 0802, 0803, and 0814. The problem is
spread over many date codes, that's why we looked at the soldering aspect of
the problem first. The last run of this board had the same problem, but
previous runs (on the same PCB batch) didn't.
We thought about "black pad" as has been suggested in some of the feedback,
but quickly removed that from the possibilities as typically the "black pad"
syndrome doesn't just affect one section of a board (particularly one device
location). And our PCB supplier is pretty solid in the ENIG department.
The failure symptom is not based on a process defect. The affected boards
(completed assemblies) fail functional test. But, when the QFP leads are
reflowed with wire solder and a little flux, they pass functional test 95%
of the time. And, as I said before, the solder junctions look like a
"Target" condition right out of IPC-A-610 before they're reflowed with wire
solder.
We're still scratching our heads on this, but are touching up each QFP until
we find the root cause - since it appears to be the only solution at this
point.
Thanks for your feedback!
Dale Ritzen, CQA
Quality Manager/ISO Management Representative
Austin Manufacturing Services
Voice: (512) 651-5338 Fax: (512) 491-7412
Email: [log in to unmask]
-----Original Message-----
From: Kane, Amol (349) [mailto:[log in to unmask]]
Sent: Wednesday, July 23, 2008 7:08 AM
To: [log in to unmask]
Subject: Re: [TN] They solder well... But they don't work!
What is the MSL on these parts? Have they been stored properly (MBB,
desiccant and HIC?) We had a similar phenomenon happen here not too long ago
and baking the parts prior to assembly improved the yield to over 95%
-Amol
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Guy Ramsey
Sent: Tuesday, July 22, 2008 10:06 AM
To: [log in to unmask]
Subject: Re: [TN] They solder well... But they don't work!
I had this experience once when I was QA Manager.
I walked into a techroom to observe a technician strum the leads of a QFP
with a dental pick. "Hear the difference?" This one will work fine now (He
was an accomplished musician and gave guitar lessons after hours). He
explained that he had just reflowed these with his solder pencil.
It turned out that there was nothing wrong with the soldering process. The
QFP was a logic array that needed to be programmed. The program did not have
a CRC. There was a timing problem. The programmer passed all parts, even if
there were errors in the download to the part.
Once we added a CRC we found that about half the parts failed to program
properly the first time. Reflowing the part and retrying while they were
warm from rework a much higher percentage accepted the program.
Fixing the clocking problem resulted in nearly 100% pass with both cool and
warm parts. It took many weeks of tossing the problem back and forth over
the wall from production to design to finally identify the root cause of the
problem . . . Bad code and a clocking problem.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Dale Ritzen
Sent: Tuesday, July 22, 2008 8:44 AM
To: [log in to unmask]
Subject: [TN] They solder well... But they don't work!
Importance: High
Here's a good one for the collective "mind-meld"...
We have a two-sided, non-RoHS compliant, all-SMT assembly (no PTH parts)
that is reflowed under a leaded profile (cooler reflow temperatures than
Pb-free). There is one 44-pin QFP on the topside of the board that
consistently solders well (i.e. passes all IPC-A-610 Class 2 inspection
criteria), but fails test until it is reflowed with a hand iron, a little
flux and wire solder. We have about a 25% pass rate without reflowing the
QFP. That jumps to around 95% once the QFP is reflowed. Several different
date codes of the device have been tried with similar results.
Thinking the ENIG pads under the device leads might be contaminated, we
cleaned them on several test case 4-up panels, with no change in yield.
Thinking it might be contaminated leads on the devices, our process guys
gently scraped off the tinned coating on the leads of several devices and
took it down to the Beryllium Copper finish. Same resultant yield.
We've re-run the failing assemblies through a higher reflow temperature with
extra "tacky flux" on them, trying to get a better reflow and use the action
of the flux to purge any contamination that might be interfering in the
solder junction. When done, the solder junctions on the device look like a
"Target - Class 1,2,3" picture from IPC-A-610, but the yield is still around
25% unless we reflow the junctions with an iron, some flux and wire solder.
There may be some things we're overlooking, but it's coming down to where we
believe the wire bonds to the lead frame material could be the source of the
problem. The intense, direct heat of the soldering iron might be enough to
generate a reflow of the wire bond, resolving any bonding issues. But, on
several different date codes? I will be getting the vendor involved shortly
to test the devices and see if they come up with something. I'm fairly
skeptical about doing this as typically the normal answer I get is "all is
working as designed".
We are all scratching our heads on this one... Any "words from the wise"
would be appreciated!
Thanks!
Dale Ritzen, CQA
Quality Manager/ISO Management Representative Austin Manufacturing Services
Email: [log in to unmask]
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet
NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send
e-mail to [log in to unmask]: SET Technet Digest Search the archives of
previous posts at: http://listserv.ipc.org/archives Please visit IPC web
site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet
NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send
e-mail to [log in to unmask]: SET Technet Digest Search the archives of
previous posts at: http://listserv.ipc.org/archives Please visit IPC web
site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
WARNING: Export Control
This document may contain technical data within the definition of the
International Traffic in Arms Regulations (ITAR), and subject to the Export
Control Laws of the U.S. Government. Transfer of such data by any means to
a foreign person, whether in the United States or abroad, without proper
export authorization or other approval from the U.S. Department of State is
prohibited.
CONFIDENTIALITY NOTICE:
This e-mail, and any attachments, is for the sole use of the intended
recipient(s) and may contain information that is confidential and protected
from disclosure under the law. Any unauthorized review, use, disclosure, or
distribution is prohibited. If you are not the intended recipient, please
contact the sender by reply e-mail, and delete/destroy all copies of the
original message and attachments.
Thank you.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet
NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send
e-mail to [log in to unmask]: SET Technet Digest Search the archives of
previous posts at: http://listserv.ipc.org/archives Please visit IPC web
site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|