Hi Amol,
First, I would suggest you use a different lab in the future, or get them
educated. The statements: " The presence of intermetallic at the interface shows
that a “Black Pad” condition is not present." is pure nonsense.
Essentially, but not exclusivley, 'Black Pad' requires that IMCs are formed—th
at enriches the P-content at the Ni/IMC interface.
Second, the fact that you have 3 different failure modes—pad cratering,
brittle interfacial separation, & BGA-side cracks, occuring, sometimes in
combination, shows that you do not have a significant weak link. Some of the
RoHS-capable PCB base materials are more brittle with lower cohesive strength, but
seeing multiple failure modes indicates that is not the issue.
Third, you do not tell me what other processes follow reflow—however,
whatever it is puts significantly higher stresses on the SAC-SJs than on the
SnPb-SJs.
CONCLUSION: The root cause is obvious—it is the switch from SnPb to SAC and
ALL that entails.
CRITICAL DIFFERENCES: A) SAC is about 40% stiffer than SnPb=>higher stresses;
B) delta-T to Tg of SAC Solidus v. SnPb Solidus is more than double=>higher
stresses;
C) delta-T to Tg of SAC Soldering T's v. SnPb Soldering T's is more than 50%
higher causing more warpage=>higher stresses;
D) SAC creep rates are about 50x slower than SnPb=>higher stresses.
I would suggest attending my new workshop Pb-Free Soldering Processes—
Survival, Quality, Reliability.
Werner
Future workshops:
Pb-Free Soldering Processes—Survival, Quality, Reliability, July 17/18, Thal,
Switzerland
Pb-Free Soldering Processes—Survival, Quality, Reliability, August 18,
Orlando
Reliability Issues with Lead-Free Soldering Processes, September 22,
Schaumburg
Failure Mode and Root Cause Analyses Reliability (Fatigue, Brittle Fracture,
ENIG), September 22, Schaumburg
Solder Joint Reliability: Parts 1 & 4, Oct. 9, Moscow, Russia
Solder Joint Reliability: Parts 1 & 4, Oct. 17, Timisoara, Rumania
Solder Joint Reliability: Parts 1 & 4, Oct. 22, Tallinn, Estonia
**************
Gas prices getting you down? Search AOL Autos for fuel-efficient used cars.
(http://autos.aol.com/used?ncid=aolaut00050000000007)
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|