I think you are talking about two different effects Black Pad and
Brittle Fracture, as one phenomenon, even though they are two completely
different things. BP isn't a (life)time variable effect, while BF is.
Of cause cratering has nothing to do with BP. It just serves as an
indicator in that particular case, that the solder joints are healthy
from the UTS point of view.
There is one observation, though; Amol mentioned I'm a bit concerned
with. He saw "...a rough Ni surface". I'm wondering whether the layer of
Ni cavitated or not.
Regards,
Vladimir
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Stadem, Richard D.
Sent: Wednesday, June 18, 2008 2:10 PM
To: [log in to unmask]
Subject: Re: [TN] [LF] [TN] SN100 for Reflow Application
No it doesn't. BP is a time-variable defect.
But I agree that it probably isn't BP, more likely a CTE mismatch issue
due to improper cooling. However, it can be both. The pad cratering has
nothing to do with BP or vice versa.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Igoshev, Vladimir
Sent: Wednesday, June 18, 2008 12:37 PM
To: [log in to unmask]
Subject: Re: [TN] [LF] [TN] SN100 for Reflow Application
Not at all. The fact that you also got cracks in laminate rules out BP
:-)
Regards,
Vladimir
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Kane, Amol (349)
Sent: Wednesday, June 18, 2008 12:51 PM
To: [log in to unmask]
Subject: Re: [TN] [LF] [TN] SN100 for Reflow Application
Dear Valdimir,
Can you please clarify your E-mail below? Do you think I may be dealing
with black pad?
Regards,
From: Igoshev, Vladimir [mailto:[log in to unmask]]
Sent: Wednesday, June 18, 2008 10:55 AM
To: [log in to unmask]; Kane, Amol (349)
Subject: Re: [LF] [TN] SN100 for Reflow Application
Hi Amol,
The thickness of intermetallic layer does not indicate whether you might
deal with BP or not, but the fact that you got laminate cracks does.
Regards,
Vladimiir
----- Original Message -----
From: Leadfree <[log in to unmask]>
To: [log in to unmask] <[log in to unmask]>
Sent: Wed Jun 18 10:33:12 2008
Subject: Re: [LF] [TN] SN100 for Reflow Application
Hi Pete,
We will not be using the DICY cured laminate in a LF process. It wont
withstand LF process temperatures. yes, we did observe a P rich area and
a rough Ni surface. However, a presence of a thick intermetallic layer
rules out black pad. it does reflect a plating bath that Is potentially
unbalanced wrt the chemical composition. However, the SnPb version of
the board is also ENIG and from the same board supplier. Therefore all
things being equal (plating wise), we see cracks only with the LF
assembly.
All the obvious SMT process steps (Solder deposition, solder ht, reflow
temps etc.,) were checked to ensure accuracy.
Regards,
Amol
-----Original Message-----
From: Pete Houwen [mailto:[log in to unmask]]
Sent: Wednesday, June 18, 2008 9:53 AM
To: [log in to unmask]; Kane, Amol (349)
Subject: Re: [TN] SN100 for Reflow Application
Amol,
If you are joints that much more prone to failure, don't rule out your
process just because they aren't failing during the process.
Are these ENiG plated boards? When you did your cross sections, did you
do any analysis of the interfacial? Are you getting P-enriched zones?
Are there voids - large or micro, in the joints or balls? Are the
soldermask openings and registration the same on both versions? Do you
inspect the paste deposition to make sure the stencil is releasing the
lead free solder as it did with tin/lead?
While the fractures aren't showing up until you apply mechanical stress,
the process itself could be weakening the joints, and that doesn't
always show up on all of the balls, or even the same ones consistently.
Though pad cratering indicates that at least at those pads, the joint
was stronger than the laminate.
Be careful using dicy cured epoxies with lead free process temperatures.
A
whole 'nother can o' worms.
Pete
WARNING: Export Control
This document may contain technical data within the definition of the
International Traffic in Arms Regulations (ITAR), and subject to the
Export Control Laws of the U.S. Government. Transfer of such data by
any means to a foreign person, whether in the United States or abroad,
without proper export authorization or other approval from the U.S.
Department of State is prohibited.
CONFIDENTIALITY NOTICE:
This e-mail, and any attachments, is for the sole use of the intended
recipient(s) and may contain information that is confidential and
protected from disclosure under the law. Any unauthorized review, use,
disclosure, or distribution is prohibited. If you are not the intended
recipient, please contact the sender by reply e-mail, and delete/destroy
all copies of the original message and attachments.
Thank you.
------------------------------------------------------------------------
-------Leadfee Mail List provided as a service by IPC using LISTSERV
1.8d To unsubscribe, send a message to [log in to unmask] with following
text in the BODY (NOT the subject field): SIGNOFF Leadfree To
temporarily stop/(start) delivery of Leadree for vacation breaks
send: SET Leadfree NOMAIL/(MAIL)
Search previous postings at: http://listserv.ipc.org/archives Please
visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
------------------------------------------------------------------------
-------
WARNING: Export Control
This document may contain technical data within the definition of the
International Traffic in Arms Regulations (ITAR), and subject to the
Export Control Laws of the U.S. Government. Transfer of such data by
any means to a foreign person, whether in the United States or abroad,
without proper export authorization or other approval from the U.S.
Department of State is prohibited.
CONFIDENTIALITY NOTICE:
This e-mail, and any attachments, is for the sole use of the intended
recipient(s) and may contain information that is confidential and
protected from disclosure under the law. Any unauthorized review, use,
disclosure, or distribution is prohibited. If you are not the intended
recipient, please contact the sender by reply e-mail, and delete/destroy
all copies of the original message and attachments.
Thank you.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|