Steve,
You may wish to take one assembly that is failing for the
high-resistance shorting under the BGA connector, and clean it. I would
try using a direct hot de-ionized water spray with a good surfactant in
the water (7% - 13%) and spray it directly at an angle underneath the
BGA connector. Follow that with an IPA rinse, and then a final
de-ionized water rinse. Blow dry the assembly with clean air to remove
all residual water/alcohol, then test again and see if the problem
disappears.
If that fixes the problem, then I would have to assume the no-clean flux
residues are the culprit. If the BGA connectors are purely mechanical,
you may wish to try cleaning them in an ultrasonic wash process prior to
assembly, again using de-ionized water heated to about 145 deg.
FAHRENHEIT, with the same 7%-13% saponifier, followed by a pass through
the wash and thorough drying. ONLY DO A SMALL QUANTITY and qualify the
process first. But do not attempt to clean the assemblies using
ultrasonics; damaged components could result.
Later, after assembly and reflow, your water-wash flux should completely
clean away in a normal in-line or batch water wash process, as it will
not have any of the no-clean flux mixed in. I do know from experience
that if you mix certain fluxes, such as Kester no-clean and Alpha
water-soluble for example, you end up with a sticky, hard conductive
residue after reflow that is difficult to completely clean away. The
alcohol reacts with the water soluble flux, and the water reacts with
the no-clean flux, producing the worst of both worlds.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Kane, Joseph E (US
SSA)
Sent: Friday, April 11, 2008 10:11 AM
To: [log in to unmask]
Subject: Re: [TN] Possible flux contamination issue
I can see how no-clean residue on the part could soften during reflow,
allowing highly active ionics from the water soluble flux to mix in and
become entrapped in the rosin (or resin, or whatever) matrix. The
result would be a a highly active residue that could be very tough to
clean.
-Joe
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Brian Ellis
Sent: Friday, April 11, 2008 10:15 AM
To: [log in to unmask]
Subject: Re: [TN] Possible flux contamination issue
A quick answer is that mixing flux types is generally a no-no! You have
no idea what the reactions may be between the two fluxes.
Brian
Steve Kelly wrote:
> Good Morning,
>
> We are assembling a BGA connector onto a flex circuit. The BGA has
> leaded balls and the BGA manufacturer uses a no-clean process to
> attach the balls to the connector and does not clean afterwards.
>
> When we assemble the BGA connector to the flex we use water soluble
> paste and then we clean. After damp heat cycling we have seen some
> shorts. When we take off the connector we see flux residues on the
> underside of the connector but not on the flex. So my question is -
> what are the concerns about mixing no-clean and water soluble? Is the
> failure likely due to inadequate cleaning or is there something else I
should be concerned about.
> I realize this is probably not the way it should be done but some days
> you just do what the customer wants - good or bad. Thanks in advance.
> Steve Kelly
>
>
>
> Steve Kelly
>
> (416) 750-8433 (work)
>
> (416) 750-0016 (fax)
>
> (416) 577-8433 (cell)
>
>
>
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
> unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt
> or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET
> Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
> posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
> archives of previous posts at: http://listserv.ipc.org/archives Please
> visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at
> [log in to unmask] or 847-615-7100 ext.2815
> -----------------------------------------------------
>
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|