Are the voids in the glass bundle or between the glass bundle and the resin?
If the former, you have a glass supplier problem (not all the weaving
assistant burned off?)-- if the latter, then I would suspect incorrect pH in the
adhesion promoter application bath.
Bill Kenyon
Global Centre Consulting
3336 Birmingham Drive
Fort Collins, CO 80526
Tel: 970.207.9586 Cell: 970.980.6373
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------